The Study on Heat Treatment Microstructure and Properties of Extruded Al-Mg-Si-Mn-Cr-Zr Alloy

Zhaoxun Cao, Jungang Han, Chen Liu, Li Lei, Jun Wang, Song Yun-kun, Yongdong XuJournal of Physics Conference Series 2023 · DOI

Abstract

In order to obtain a high-strength Al-Mg-Si aluminum alloy with a tensile strength of more than 400MPa, a trace amount of Zr is added to the 6082 aluminum alloy to obtain an Al-1.0Mg-1.05Si-0.55Mn-0.15Cr-0.045Zr alloy. The mechanical properties and microstructure of the extruded alloy were studied by tensile performance test, metallography, scanning electron microscope (SEM), transmission electron microscope (TEM), electron backscatter diffraction (EBSD) observation and energy spectrum analysis. The results show that, after 545°C×2h+170°C×8h heat treatment, the alloy has the best mechanical properties. The tensile strength, yield strength and elongation at break reached 423MPa, 402MPa and 14%, respectively. The alloy strengthening mechanism is mainly due to the large number of dispersed needle-like β″ phases, sub-micron α-Al(MnCrFe)Si phases, α-Al(MnFe)Si phases and micron-level α-Al(MnCrFe)Si phases precipitated inside the grains and grain boundaries. The average grain size of the alloy is 7.41μm, and a bimodal grain structure composed of low-angle grain boundaries and high-angle grain boundaries is formed.

Introduction

As the automotive industry shifts toward New Energy Vehicles (NEVs), weight reduction has become a critical engineering priority. Al-Mg-Si (6xxx series) alloys are widely utilized for their corrosion resistance and weldability, but standard grades often struggle to meet the high-strength requirements (tensile strength > 400 MPa) needed for load-bearing components like automotive control arms. This study investigates how a specific chemical modification—adding Mn, Cr, and trace Zr—combined with optimized heat treatment, can push the performance boundaries of extruded aluminum alloys.

Experimental Methods

The research focused on an extruded Al-1.0Mg-1.05Si-0.55Mn-0.15Cr-0.045Zr alloy bar. To identify the optimal processing window, samples were subjected to five different solution treatment temperatures ranging from 535°C to 575°C for 2 hours, followed by water quenching and a standard aging cycle of 170°C for 8 hours. The resulting microstructures were analyzed using SEM, TEM, and EBSD to map grain orientations and identify the chemical makeup of intermetallic phases.

Results and Discussion

The 545°C "Sweet Spot"

Mechanical properties peaked at a solution temperature of 545°C. As shown in the microhardness data, there is a clear peak in hardness at this temperature before a decline at higher thermal levels.

Microhardness (HV) as a function of solution treatment temperature (T/°C).

At the 545°C threshold, the alloy achieved its peak tensile strength of 423 MPa and a yield strength of 402 MPa. Moving to higher temperatures (e.g., 575°C) caused a decline in strength because the precipitation-free zones (PFZs) at the grain boundaries widened and precipitates began to aggregate, losing their strengthening efficiency.

Tensile strength (TS), yield strength (YS), and elongation (A) vs. solution treatment temperature.

Multi-Scale Strengthening and Grain Architecture

The alloy's strength is derived from a hierarchy of precipitates. Nano-scale needle-like β″ phases (20-80 nm) provide the primary barrier to dislocation movement, while sub-micron and micron-scale α-Al(MnCrFe)Si phases contribute to dispersion strengthening.

Furthermore, the extrusion and heat treatment resulted in a bimodal grain structure with an average grain size of 7.41 μm. The alloy retained a mix of low-angle grain boundaries (31.6%) and high-angle boundaries (41.5%), which helps maintain a balance between high strength and a respectable 14% elongation. Trace Zr (0.045%) played a vital role in refining this structure and stabilizing the alloy against excessive grain growth during high-temperature solutionizing.

Conclusion

By optimizing the solution treatment temperature to 545°C, researchers successfully engineered a modified 6082 alloy that exceeds the 400 MPa tensile strength threshold. The combination of trace Zr and a precise thermal window creates a dense forest of needle-like β″ precipitates and a stable bimodal grain structure, offering a promising material solution for high-strength, lightweight automotive components.

Summary updated

Abstract

Abstract In order to obtain a high-strength Al-Mg-Si aluminum alloy with a tensile strength of more than 400MPa, a trace amount of Zr is added to the 6082 aluminum alloy to obtain an Al-1.0Mg-1.05Si-0.55Mn-0.15Cr-0.045Zr alloy. The mechanical properties and microstructure of the extruded Al-1.0Mg-1.05Si-0.55Mn-0.15Cr-0.045Zr alloy were studied by tensile performance test, metallography, scanning electron microscope (SEM), transmission electron microscope (TEM), electron backscatter diffraction (EBSD) observation and energy spectrum analysis. The results show that, after 545°C×2h+170°C×8h heat treatment, the alloy has the best mechanical properties. The tensile strength, yield strength and elongation at break reached 423MPa, 402MPa and 14%, respectively. The alloy strengthening mechanism is mainly due to the large number of dispersed needle-like β′ phases, sub-micron α-Al(MnCrFe)Si phases, α-Al(MnFe)Si phases and micron-level α-Al(MnCrFe)Si phases precipitated inside the grains and grain boundaries. The alloy precipitates sub-micron α-Al(MnCrFe)Si phase, α-Al(MnFe)Si phase and micron-level α-Al(MnCrFe)Si phase. After the alloy is treated at 545°C×2h+170°C×8h, a large number of dispersed needle-like β″ precipitations are uniformly precipitated in the inside the grains respectively. These precipitations can improve the strength of the material. The average grain size of the alloy is 7.41μm, and a bimodal grain structure composed of low-angle grain boundaries and high-angle grain boundaries is formed.
BibTeX
@article{cao2023study,
  author = {Zhaoxun Cao and Jungang Han and Chen Liu and Li Lei and Jun Wang and Song Yun-kun and Yongdong Xu},
  title = {{The Study on Heat Treatment Microstructure and Properties of Extruded Al-Mg-Si-Mn-Cr-Zr Alloy}},
  journal = {Journal of Physics Conference Series},
  year = {2023},
  doi = {10.1088/1742-6596/2478/12/122006},
}
Figure