Abstract
A series of as-cast lightweight multicomponent alloys Al(86-x)Mg10Zn2Cu2Six (x=0, 0.3, 0.6, 0.9, 1.2 at.%) were prepared by a vacuum induction furnace with a steel die. With the addition of Si, the reticular white Al-Cu phase deposited were gradually replaced by the gray eutectic Mg-Si phase, while the compressive strength of the alloys increases first and then decreases slowly. It is particularly noteworthy that the compression plasticity also exhibits this trend. When the Si content is 0.9 at.%, the compressive strength reaches its maximum at 779.11 MPa and the compressive plasticity reaches 20.91%. The effect of the addition of Si on the serration behavior of alloy was also studied; we found that the addition of Si introduces a new MgSi phase, and with the change of Si is significantly affects the morphology of the precipitated phase, which affects the serration behavior of the alloys. The comprehensive mechanical properties of the alloy are optimal at the critical point where the serration behavior disappears. In this work, we have provided a method and a composition for the preparation of a low-cost, high-strength, lightweight medium-entropy alloys.
Introduction
As global industries prioritize energy efficiency, the demand for lightweight, high-strength materials has intensified. While traditional aluminum and magnesium alloys are industry standards, researchers are increasingly exploring High-Entropy Alloys (HEAs) and Medium-Entropy Alloys (MEAs) to surpass existing performance limits. However, many HEAs utilize dense elements like Cobalt or Nickel, making them unsuitable for weight-sensitive transport applications. Furthermore, these alloys often exhibit "serrated flow" (the Portevin-Le Chatelier effect)—unstable, jerky plastic deformation that can lead to premature failure and poor surface finishes. This study investigates the design of a lightweight MEA that balances strength, ductility, and deformation stability through trace Silicon (Si) additions.
Experimental Methods
The research team synthesized five alloy compositions based on the formula $Al_{(86-x)}Mg_{10}Zn_2Cu_2Si_x$ ($x = 0, 0.3, 0.6, 0.9, 1.2$ at.%). The alloys were melted in a vacuum induction furnace and cast into 30mm cylindrical steel dies.
Microstructural characterization was performed using Scanning Electron Microscopy (SEM) and Energy Dispersive Spectroscopy (EDS) for elemental mapping, while Electron Backscattered Diffraction (EBSD) was employed to determine grain size. Phase identification was conducted via X-ray Diffraction (XRD). Mechanical performance was evaluated through standard compression tests and Vickers micro-hardness measurements to correlate internal structure with macroscopic properties.
Results and Discussion
Microstructural Evolution
Adding Silicon fundamentally alters the alloy's microstructural "skeleton." The addition of Si facilitates a phase shift where the reticular white Al-Cu phase is progressively replaced by a gray eutectic Mg-Si phase. At the optimal concentration of 0.9 at.% Si, a significant volume of lamellar eutectic structures forms, promoting easier dislocation glide and enhanced plasticity.
Mechanical Properties and Serration Suppression
The alloy containing 0.9 at.% Si demonstrated peak performance, achieving a maximum compressive strength of 779.11 MPa and a compressive plasticity of 20.91%. Micro-hardness followed a similar trend, peaking at this composition. EBSD analysis confirmed a refined grain size (200–300 μm) for this optimal alloy.
Crucially, the 0.9 at.% Si addition suppressed serrated flow. Serrations typically arise from "Dynamic Strain Aging," where solute atoms like Magnesium pin dislocations. Silicon effectively "scavenges" Magnesium from the solid solution to form $Mg_2Si$ precipitates, reducing the concentration of free Magnesium in the matrix and smoothing the material's flow. However, exceeding this threshold (e.g., 1.2 at.% Si) introduced casting defects such as pores, leading to a decline in mechanical properties.
Conclusion and Future Outlook
This research identifies 0.9 at.% Si as a critical threshold for optimizing the performance of lightweight Al-Mg-Zn-Cu MEAs. This specific addition maximizes strength and ductility while eliminating unstable flow. Future work should focus on optimizing the casting process to eliminate porosity at higher Si concentrations, exploring heat treatments to further refine precipitates, and conducting tensile testing to fully validate these materials for structural applications.
Summary updated