Abstract
This study details the successful scale-up of electroslag remelting (ESR) to produce 50-ton steel slabs with cross-sections up to 960×2000 mm. By integrating low-frequency power, optimized five-component slag systems, and advanced atmospheric shielding, researchers achieved ultra-thick plates suitable for high-stress applications like hydropower stations. These slabs exhibit superior internal quality, low impurity levels, and isotropic mechanical properties that surpass traditional continuous or ingot casting methods.
Introduction
The growing demand in nuclear power, offshore engineering, and hydropower for "super-thick" steel plates (150–400 mm) has pushed traditional manufacturing to its limits. Continuous casting often fails to maintain internal quality and control segregation at thicknesses exceeding 350 mm. While traditional ingot casting can reach these dimensions, the resulting metal frequently suffers from poor macrostructure and weak through-thickness (Z-direction) properties. This paper explores the optimization of the Electroslag Remelting (ESR) process to produce large-scale, high-purity slabs that require minimal forging and offer exceptional mechanical consistency.
Methodology and Experimental Setup
The research utilized 50-ton ESR furnaces featuring several technical innovations designed to optimize efficiency and quality.
Electrical and Mechanical Systems
A low-frequency power source (0.1–5 Hz) combined with a bifilar electrode connection was employed to reduce inductive resistance and increase the power factor. This setup ensures a stable load on the three-phase grid while lowering energy consumption. The furnaces utilize a mobile mold (crystallizer) and secondary compressed-air cooling to accelerate solidification, which is critical for refining the grain structure in such massive ingots.
Slag Engineering and Atmospheric Control
The team developed complex five-component slag systems ($CaF_2-Al_2O_3-CaO-SiO_2-MgO$). A primary goal was identifying "long slags"—those exhibiting a gradual change in viscosity over temperature—to ensure smooth slab surfaces during the relative movement of the mold. To mitigate hydrogen embrittlement and oxidation, the process was conducted within a protective housing supplied with ultra-dry air (dew point below –40 °C) and optimized argon shielding, the latter designed using FLUENT fluid dynamics modeling.
Results and Discussion
Slag Performance and Hydrogen Management
Analysis of the slag systems revealed that slag S2, with the highest $SiO_2$ content, functioned effectively as a "long slag." This characteristic prevents abrupt viscosity jumps, which is vital for maintaining surface integrity in large-scale remelting.
Furthermore, while $CaO$ improves refining, it also increases hydrogen permeability. The researchers managed this by using pre-melted slag and a "hot start" (40% liquid/60% solid flux) under a dry air blanket, successfully keeping hydrogen levels within strict limits despite the 42-hour remelting duration.
Metallurgical Quality and Mechanical Properties
The ESR process yielded significant improvements:
- Yield and Purity: Metal yield increased by 9–18% compared to traditional casting by reducing the need for extensive cropping and forging. Oxygen and nitrogen levels were kept remarkably low (~0.0010% and ~0.0050%, respectively), with non-metallic inclusion ratings consistently at 0 or 0.5.
- Isotropy: A major achievement was the near-elimination of anisotropy. In a 265 mm thick S500Q/Z35 steel plate, yield strength remained stable (470–480 MPa) throughout the thickness.
- Toughness: The material demonstrated excellent low-temperature toughness, with a ductile-to-brittle transition temperature (DBTT) of approximately –40 °C. High impact energy values in the Z-direction confirm the structural integrity provided by the bifilar ESR approach.
Conclusion
The optimized ESR process successfully produces massive, high-quality steel slabs that meet the rigorous demands of modern heavy industry. While the 42-hour production cycle necessitates stringent atmospheric controls to prevent hydrogen absorption, the resulting metallurgical purity and isotropic mechanical properties represent a significant advancement over traditional casting methods. Future efforts will focus on further refining melting rates to balance productivity with the fine-grained structures required for plates exceeding 400 mm in thickness.