Abstract
In this study, EH36 is thick steel plate, which welded by auto <TEX>$CO_2$</TEX> gas welding machine, has been applied on offshore filed. The specimen was examined by indentation tester and it was measured for fracture toughness at <TEX>$18^{\circ}C$</TEX>, <TEX>$0^{\circ}C$</TEX>, <TEX>$-20^{\circ}C$</TEX> and <TEX>$-45^{\circ}C$</TEX> by low temperature chamber, respectively. The absorbed energy was got on same temperature by Charpy impact tester. The weld surface was observed for watch of changed crystalline structure by optical microscope, and fracture surface of impact test specimen were observed by scanning electron microscope(SEM).
Introduction
Offshore structures, including oil platforms and large container vessels, are increasingly operating in extreme environments such as polar regions. These structures rely heavily on high-strength steels like EH36. However, the welding processes required for construction create Heat Affected Zones (HAZ) and introduce residual stresses that can lead to brittle failure at low temperatures.
Traditionally, material integrity is assessed using destructive methods like the Charpy Impact Test or Crack Tip Opening Displacement (CTOD). While these provide accurate data, they require the removal of large material samples, making them unsuitable for in-situ structural health monitoring. This study investigates the use of instrumented indentation as a semi-non-destructive alternative to evaluate the mechanical properties of welded EH36 plates under sub-zero conditions.
Experimental Methodology
The research utilized 40mm thick EH36 steel plates joined via a multi-pass auto-welding process using $CO_2$ gas. The weld joint geometry was designed with a 70-degree groove angle to accommodate five distinct welding passes, ensuring full penetration and structural integrity.
Mechanical evaluation was performed using the AIS3000 instrumented indentation system. Unlike conventional hardness testing, this equipment records a continuous load-depth curve, allowing for the calculation of yield strength, tensile strength, and fracture toughness. To simulate arctic conditions, the tester was integrated with a high-low temperature chamber capable of reaching $-45^{\circ}C$ using liquid nitrogen cooling.
Validation of the indentation results was conducted through traditional Charpy impact tests and microstructural analysis using Scanning Electron Microscopy (SEM) to observe fracture surfaces at varying temperatures.
Results and Discussion
Strength and Depth Profiles
The study revealed that the weld metal possesses significantly higher strength compared to the base metal. Specifically, the base metal yield strength was measured at 294 MPa, whereas the weld metal reached 345 MPa. Interestingly, yield strength increased with depth within the weld, peaking at 396 MPa at a depth of 20mm. This phenomenon is attributed to the "reheating effect," where subsequent welding passes act as a localized heat treatment for underlying layers, refining the grain structure and enhancing strength.
Low-Temperature Fracture Toughness
Fracture toughness measurements across temperatures of $18^{\circ}C$, $0^{\circ}C$, $-20^{\circ}C$, and $-45^{\circ}C$ showed a clear degradation in material properties as temperatures dropped. A critical transition was observed around $-20^{\circ}C$, where the material began shifting from ductile to brittle behavior. At $-45^{\circ}C$, the absorbed energy of the base metal dropped significantly to approximately 150 J from its peak of 235 J at $0^{\circ}C$.
The HAZ demonstrated relatively stable absorbed energy across the temperature range. This stability is likely due to the formation of acicular ferrite during the rapid thermal cycles of welding, which provides resistance to crack propagation.
Microstructural Confirmation
SEM analysis of the fracture surfaces confirmed these findings. At room temperature, the surfaces exhibited "dimples" characteristic of ductile tearing. In contrast, specimens tested at $-45^{\circ}C$ showed flat, crystalline "cleavage" facets, indicating a complete transition to brittle fracture.
Conclusion
The results demonstrate that instrumented indentation testing using the AIS3000 system provides a reliable correlation with traditional destructive testing methods. It successfully captured the strength variations across the weld depth and the brittle transition behavior at low temperatures. This approach offers a viable, semi-non-destructive tool for the on-site evaluation of offshore structures, potentially improving safety and maintenance efficiency in extreme environments.
Summary updated