Electrical and Optical Properties of Sb-doped SnO2Thin Films Fabricated by Pulsed Laser Deposition

Ki-Sun Jang, Jungwoo Lee, Joongwon Kim, Sang‐Im YooJournal of the Korean Ceramic Society 2014 · DOI

Abstract

We fabricated undoped and Antimony (Sb)-doped tin oxide ($SnO_2$) thin films on glass substrates using a pulsed laser deposition (PLD) process. High-density targets (~90%) were prepared via spark plasma sintering (SPS) to overcome the traditional sintering challenges of tin oxide. We investigated the effects of deposition temperature (100–600°C) and Sb doping concentration (2–8 wt%) on the material's performance. Undoped films achieved their lowest resistivity at 200°C due to oxygen vacancies. However, the 2 wt% Sb-doped film deposited at 400°C emerged as the optimal configuration, exhibiting a low resistivity of $5.43 \times 10^{-3} \Omega \cdot cm$, a high average transmittance of 85.8%, and a superior Figure of Merit of 1202. These results position Sb-doped $SnO_2$ as a robust, cost-effective alternative to Indium Tin Oxide (ITO).

Introduction

Transparent Conducting Oxides (TCOs) are essential for modern optoelectronics, including touchscreens, flat-panel displays, and solar cells. While Indium Tin Oxide (ITO) is the current industry standard, its high cost, chemical instability in harsh environments, and mechanical fragility limit its long-term viability. Tin oxide ($SnO_2$) is a promising alternative due to its abundance, chemical robustness, and mechanical strength. This study focuses on optimizing the electrical and optical properties of $SnO_2$ through precise Sb doping and temperature control using Pulsed Laser Deposition (PLD).

Experimental Methods

Targets with varying $Sb_2O_3$ concentrations (0–8 wt%) were synthesized using Spark Plasma Sintering (SPS) at 1000°C, achieving approximately 90% of the theoretical density. Thin films were subsequently grown on glass substrates using a KrF excimer laser PLD system. The substrate temperature ($T_s$) was varied from 100°C to 600°C to evaluate its impact on crystallinity and carrier dynamics. The resulting films were characterized using X-ray diffraction (XRD), field-emission scanning electron microscopy (FE-SEM), Hall effect measurements, and UV-Vis spectroscopy.

Results and Discussion

Temperature Effects on Undoped Films

The electrical performance of undoped $SnO_2$ is primarily governed by oxygen vacancies. As shown in Figure 3, the resistivity of undoped films reaches a minimum at a substrate temperature of 200°C. At this temperature, the carrier concentration is maximized. As the temperature increases further to 400°C and 600°C, the films become more stoichiometric and crystalline, which reduces the number of oxygen vacancies and subsequently increases resistivity.

Electrical properties (resistivity, carrier concentration, and mobility) of undoped SnO2 films as a function of substrate temperature (Ts).

Optimization via Antimony Doping

To improve conductivity beyond the limits of oxygen vacancies, Antimony was introduced as a dopant. $Sb^{5+}$ ions substitute for $Sn^{4+}$ in the lattice, donating free electrons. The effectiveness of this substitution is highly dependent on the deposition temperature. At 400°C, the films possess sufficient crystallinity for efficient substitution.

As illustrated in Figure 5, the 2 wt% Sb-doped film deposited at 400°C (Fig. 5b) shows a significant drop in resistivity compared to the undoped sample at the same temperature. This is driven by a sharp increase in carrier concentration to $2.08 \times 10^{20} cm^{-3}$. However, increasing the doping concentration beyond 2 wt% leads to a decrease in mobility due to ionized impurity scattering, where excess antimony ions act as obstacles for electron flow.

Electrical properties of Sb-doped SnO2 films as a function of doping concentration at (a) 200°C and (b) 400°C.

Optical Performance

All films maintained high transparency in the visible spectrum. The optimized 2 wt% Sb-doped film at 400°C achieved an average transmittance of 85.8%. The researchers also observed a "blue shift" in the optical absorption edge with increased doping, a phenomenon known as the Moss-Burstein effect, where the filling of lower conduction band states necessitates higher energy for electronic transitions.

Conclusion

By combining Spark Plasma Sintering for dense target fabrication and Pulsed Laser Deposition for thin-film growth, we successfully optimized Sb-doped $SnO_2$ thin films. The 2 wt% Sb-doped film deposited at 400°C provides an excellent balance of high transparency and low resistivity, resulting in a high Figure of Merit (1202). While commercial ITO still holds a conductivity advantage, the durability and cost-effectiveness of Sb-doped $SnO_2$ make it a highly viable candidate for next-generation transparent electrodes.

Summary updated

Abstract

We fabricated undoped and Sb-doped SnO 2 thin films on glass substrates by a pulsed laser deposition (PLD) process. Undoped and 2 -8 wt% Sb 2 O 3 -doped SnO 2 targets with a high density level of ~90% were prepared by the spark plasma sintering (SPS) process. Initially, the effects of the deposition temperature on undoped SnO 2 thin films were investigated in the region of 100 -600 o C. While the undoped SnO 2 film exhibited the lowest resistivity of 1.20 10 -2 cm at 200 o C due to the highest carrier concentration generated by the oxygen vacancies, 2 wt% Sb-doped SnO 2 film exhibited the lowest resistivity value of 5.43 10 -3 cm, the highest average transmittance of 85.8%, and the highest figure of merit of 1202 -1
BibTeX
@article{jang2014electrical,
  author = {Ki-Sun Jang and Jungwoo Lee and Joongwon Kim and Sang‐Im Yoo},
  title = {{Electrical and Optical Properties of Sb-doped SnO<sub>2</sub>Thin Films Fabricated by Pulsed Laser Deposition}},
  journal = {Journal of the Korean Ceramic Society},
  year = {2014},
  doi = {10.4191/kcers.2014.51.1.043},
}
Figure