WELDING OF SUPER DUPLEX S32750 WITH DOCOL 1100 FOR THE TRANSPORT PURPOSES

Tomasz Węgrzyn, Bożena Szczucka-Lasota, Chen Feng, Katarzyna Turoń, Adam Jurek, Novar Sp. z o.o., GliwiceScientific 2023 · DOI

Abstract

This paper investigates the dissimilar welding of Super Duplex Stainless Steel (SDSS) S32750 with Advanced High-Strength Steel (AHSS) DOCOL 1100 M for automotive applications. The primary challenge lies in joining two materials with vastly different microstructures—martensite and a mixture of austenite and delta ferrite. Through a controlled experimental matrix using Metal Active Gas (MAG) welding, the study identifies optimal pre-heating temperatures and shielding gas compositions to produce high-strength, defect-free joints.

Introduction

In the automotive industry, the drive for lighter and safer vehicles necessitates the use of diverse materials. However, "dissimilar welding"—joining metals with distinct chemical and physical properties—presents significant metallurgical hurdles. Super Duplex S32750 offers excellent corrosion resistance, while DOCOL 1100 M provides extreme strength. Their differing thermal conductivities and expansion rates often lead to cracking or weakened heat-affected zones (HAZ). This research aims to find the "Goldilocks" zone of welding parameters to successfully bridge these two materials.

Materials and Methods

The researchers employed Metal Active Gas (MAG) welding with a 1 mm diameter austenitic 309LSi filler wire. The experimental design focused on two critical variables: pre-heating temperature (120°C, 150°C, and 200°C) and the nitrogen content in the shielding gas (Ar + 18% $CO_2$ with 2%, 3%, or 4% $N_2$).

Table 1: Experimental matrix of shielding gas mixtures and pre-heating temperatures for samples E1 through E9.

The resulting joints were evaluated using both non-destructive testing (NDT), such as visual and magnetic particle inspections, and destructive testing (DT), including tensile and bending tests. Chemical analysis was also performed to measure the nitrogen content in the weld metal.

Results and Discussion

The study revealed a critical relationship between pre-heating temperature and joint integrity. At a low pre-heat of 120°C, cracking was observed on the SDSS side. Conversely, a high pre-heat of 200°C led to an over-expanded HAZ on the AHSS side, compromising the martensitic structure. The optimal compromise was found at 150°C.

Furthermore, the addition of nitrogen to the shielding gas proved beneficial. Nitrogen migrates into the weld pool, increasing the Ultimate Tensile Strength (UTS) of the joint. Sample E6, utilizing a 150°C pre-heat and 4% $N_2$ shielding gas, emerged as the superior configuration.

Table 2: Summary of observations for each experimental sample, highlighting the presence of cracks or correct weld dimensions.

Key findings include:

  • Optimal Strength: Sample E6 achieved a UTS of 533 MPa, significantly higher than samples with lower nitrogen content (which often failed to reach 500 MPa).
  • Ductility: Bending tests for optimized samples showed no cracks on either the face or root, indicating a robust joint suitable for transport vibrations.
  • Quality: NDT confirmed that the 150°C/4% $N_2$ combination produced a correct HAZ form and dimension without the typical defects found in dissimilar welds.

Conclusion

Successful dissimilar welding of SDSS S32750 and AHSS DOCOL 1100 M is achievable by carefully controlling thermal input and gas chemistry. A pre-heating temperature of 150°C combined with a 4% nitrogen-enriched shielding gas produces joints that meet the rigorous demands of the transport industry. Future work may explore more complex gas mixtures and long-term fatigue performance to further validate these findings for large-scale production.

Summary updated

Abstract

The main novelty and the goal of the paper is to present the dissimilar SDSS with AHSS welding for automotive application. The welding automotive structure is connected with two different grades of steel with various structure (martensite with mixture of austenite and delta ferrite). Design/methodology/approach: Two dissimilar grades of steel were welded in order to get a proper joint for automotive industry. The properties of the joint was carefully tested (NDT and DT). Findings: Relations between various welding parameters and the properties of weld.
BibTeX
@inproceedings{wegrzyn2023welding,
  author = {Tomasz Węgrzyn and Bożena Szczucka-Lasota and Chen Feng and Katarzyna TUROŃ and Adam Jurek and Novar Sp. z o.o., Gliwice},
  title = {{WELDING OF SUPER DUPLEX S32750 WITH DOCOL 1100 FOR THE TRANSPORT PURPOSES}},
  booktitle = {Scientific},
  year = {2023},
  doi = {10.29119/1641-3466.2023.189.42},
}
Figure