Abstract
The effect of ultrasonic energy on the pretreatment and leaching of gold from refractory ore was investigated. The process involved a two-stage approach: sodium hydroxide (NaOH) pretreatment followed by cyanide leaching, both under ultrasonic intensification. Results indicated that while ultrasound significantly enhances the leaching ratio, excessive pretreatment time (beyond 1 hour) or high NaOH concentrations actually decrease gold recovery due to the formation of gold-adsorbing silica gels. Optimal conditions, including acoustic power and NaCN concentration, were identified, demonstrating ultrasound as a viable technique for extractive metallurgy in refractory gold ores.
Introduction
The mining industry increasingly relies on refractory gold ores as "free-milling" deposits become depleted. In these ores, gold is often encapsulated within minerals like pyrite or associated with organic carbon, making standard cyanide leaching ineffective. Conventional pretreatment methods like roasting or pressure oxidation are energy-intensive and environmentally costly. This study explores ultrasound-intensified leaching as a more efficient alternative, leveraging acoustic cavitation to accelerate chemical kinetics and improve mass transfer.
Methods
The experimental procedure followed a two-stage ultrasound-assisted process. Initially, the gold ore (crushed to -0.074 μm) underwent ultrasound pretreatment with NaOH to decompose shielding minerals. Subsequently, the pretreated ore was subjected to ultrasound-intensified cyanide leaching.
Analytical techniques including Atomic Absorption Spectrometry, X-ray Diffraction (XRD), and Scanning Electron Microscopy (SEM) with EDX were used to characterize the leaching ratios and mineralogical changes.
Key Insights: The "Silica Gel" Trap
A significant finding was the detrimental effect of prolonged pretreatment. Increasing the ultrasound pretreatment time from 1 to 5 hours led to a decrease in the final gold leaching ratio. XRD and SEM analyses suggested that NaOH reacts with the ore's silica content to form sodium silicate, which subsequently transforms into a silica gel. This gel physically adsorbs gold particles, rendering them inaccessible to the cyanide leaching agent in the second stage.
Results and Discussion
The application of ultrasound remarkably increased the gold leaching ratio compared to conventional methods. Without ultrasound, the leaching ratio was approximately 40.3%. With 180W ultrasound intensification, this jumped to 73.4%.
As shown in the figure above, the highest leaching ratio (~80.5%) was achieved with a 1-hour pretreatment time. Furthermore, increasing the NaCN concentration from 6 to 18 kg/t steadily improved recovery, peaking at 80.7%. The study also highlighted that excessive acoustic power (e.g., 1 kW) during the leaching stage can decompose the cyanide reagent, emphasizing the need for optimized "Goldilocks" power levels.
Conclusion
Ultrasound-intensified leaching offers a promising pathway for processing refractory gold ores. By optimizing pretreatment duration and acoustic power, researchers achieved recovery rates exceeding 80%, significantly higher than traditional leaching. While challenges remain in industrial scaling and economic optimization, the technical viability of acoustic cavitation in extractive metallurgy is clearly demonstrated.
Summary updated