Surfactant usage in nitrile rubber film development through metal plate dipping process

Le Hui, Yamuna Munusamy, Norliza Ismail, Ooi Zhong Xian, Mathialagan Muniyadi, Lim Chaw JiangE3S 2025 · DOI

Abstract

Developing rubber film in the laboratory is essential for studying mechanical changes in gloves with varying formulations. However, lab processes differ significantly from industrial manufacturing; while factories use ceramic formers in controlled environments, lab films are often formed by dipping metal plates into compounded mixtures. A significant hurdle in lab preparation is the inability of the coagulant to uniformly coat the metal plate, leading to uneven films. This study investigates incorporating surfactants into the calcium nitrate ($Ca(NO_3)_2$) coagulant solution to achieve uniform coating. Two types of surfactants at two concentrations were evaluated by measuring the contact angle on metal plates. Results indicate that 0.5% Wetpol 800 surfactant provides an even coating through visual inspection. The resulting rubber film exhibited an average thickness of 0.065 mm, tensile strength of 22.348 MPa, and ultimate elongation of 1388.4%.

Introduction

In industrial glove manufacturing, nitrile rubber is deposited onto complex ceramic "formers." In research settings, flat metal plates are preferred for developing and testing new formulations due to ease of handling. However, the standard coagulant solution, calcium nitrate, possesses high surface tension and wets metal surfaces poorly. Instead of a smooth film, the coagulant tends to "bead up" into droplets.

High contact angle of the standard coagulant solution on a metal plate, leading to non-uniform coating.

When these plates are dipped into nitrile latex, the rubber adheres only to these droplets, causing pinholes and uneven mechanical properties. This work focuses on optimizing surfactant concentrations to lower the contact angle and ensure a continuous, uniform film.

Methodology

The researchers prepared a base coagulant of 15% wt $Ca(NO_3)_2$ and tested two non-ionic surfactants: Wetpol 800 (an organosilicone "super-spreader") and Tween 20 (a common polysorbate). Each was tested at 0.005% and 0.5% wt concentrations.

Contact angles were measured by placing a droplet on a steel plate, capturing images at 10x magnification, and analyzing them using ImageJ. The dipping process involved pre-heating plates to 70°C, coagulant dipping, drying, dipping into the NBR compound (containing ZnO, sulfur, and accelerators) for 7 minutes, water leaching, and vulcanization at 100°C.

Results and Discussion

The study found that adding calcium nitrate to deionised water increased the contact angle from approximately 69° to 77°, as ions cause water molecules to aggregate. To achieve a uniform coat, the contact angle typically needs to fall below a "superhydrophilic" threshold of 40–50°.

Wetpol 800 significantly outperformed Tween 20. At a 0.5% concentration, Wetpol 800 reduced the contact angle to 32.5°, whereas 0.5% Tween 20 only reached 41.3%.

Optimized low contact angle (32.5°) achieved with 0.5% Wetpol 800, allowing for a uniform coagulant layer.

The 0.5% Wetpol 800 formulation produced rubber films that exceeded ASTM D6319 medical-grade standards:

  • Tensile Strength: 22.35 MPa (ASTM minimum: 14 MPa).
  • Ultimate Elongation: 1388.4% (ASTM minimum: 500%).
  • Uniformity: Visual inspection confirmed a smooth, hole-free coating.

Conclusion

Incorporating 0.5% Wetpol 800 into the calcium nitrate coagulant effectively bridges the gap between lab-scale experimentation and industrial quality. While successful for steel plates, future work should examine the long-term effects of residual surfactants on rubber aging and their interactions with different leaching processes or metal alloys.

Summary updated

Abstract

Developing rubber film in the lab is important for studying the mechanical changes on gloves with different developed formulation. The process in the lab differs from the factory, as the rubber film is formed from dipping a metal plate into the compounded mixture, while the factory uses a well-crafted former to make their gloves in a controlled environment. One issue arises during preparation rubber film in laboratory is the coagulant was unable to uniformly coat the metal plate, which result in producing uneven rubber films. Thus, this work focuses on the incorporation of surfactant into the coagulant solution (Ca(NO 3 ) 2 ) to allow a uniform coating. Two concentrations of two types of surfactants are tested by measuring the contact angle of coagulant to the metal plate. 0.5% of Wetpol 800 surfactant provides an even coating of rubber film on the metal plate after dipping through visual inspection compared to the Ca(NO 3 ) 2 alone. The rubber film formed has an average thickness of 0.065 mm, tensile strength of 22.348 MPa, ultimate elongation 1388.4 %, modulus E100 and E300 of 1.377 and 0.731 respectively.
BibTeX
@inproceedings{hui2025surfactant,
  author = {Le Hui and Yamuna Munusamy and Norliza Ismail and Ooi Zhong Xian and Mathialagan Muniyadi and Lim Chaw Jiang},
  title = {{Surfactant usage in nitrile rubber film development through metal plate dipping process}},
  booktitle = {E3S},
  year = {2025},
  doi = {10.1051/e3sconf/202560302009},
}
Figure