Study on the Preparation Process Optimization of Plywood Based on a Full Biomass Tannin-Sucrose Wood Adhesive

Wen Gu, Xinyue Ding, Min Tang, Feiyan Gong, Shuangshuang Yuan, Jintao DuanJOURNAL 2023 · DOI

Abstract

Biomass adhesives are essential for reducing the wood industry's reliance on fossil-based synthetic resins and achieving carbon neutrality. This study details the development and optimization of a fully bio-based wood adhesive composed of tannin and sucrose. Through systematic testing, researchers identified that hot-pressing temperature is the critical factor for performance. Under optimal conditions (220°C), the adhesive achieved a wet bonding strength of 0.83 MPa, meeting industrial Type-I plywood standards.

Introduction: The Need for Green Adhesives

The wood industry heavily relies on synthetic resins like urea-formaldehyde. While effective, these adhesives release harmful volatile organic compounds (VOCs) and contribute significantly to the industry's carbon footprint. Although bio-adhesives have emerged as alternatives, many still require petrochemical cross-linkers to achieve necessary water resistance. This research explores a 100% biomass solution using waxberry tannin and sucrose.

The Tannin-Sucrose Mechanism

The effectiveness of this adhesive relies on a specific two-step chemical reaction triggered during the hot-pressing process. First, high heat transforms sucrose into furan aldehydes, such as 5-hydroxymethylfurfural (5-HMF). Second, these aldehydes act as cross-linking agents, reacting with the polyphenol structure of the tannin to create a robust, waterproof network.

Proposed chemical reaction mechanism between tannin and sucrose.

Experimental Optimization

To determine the ideal production parameters, the researchers employed an orthogonal experimental design ($L_{16}(4^4)$). They evaluated four key variables:

  • Hot-pressing temperature: 200°C to 230°C
  • Hot-pressing time: 1.0 to 1.6 min/mm
  • Adhesive loading: 140 to 200 g/m²
  • Mass ratio (Tannin:Sucrose): 60:40 to 30:70

The resulting bonds were analyzed using Differential Scanning Calorimetry (DSC), Fourier Transform Infrared Spectroscopy (FT-IR), and X-ray Diffraction (XRD) to map the chemical and crystalline evolution of the adhesive.

Key Insights and Results

The study revealed that temperature is the gatekeeper for this bio-adhesive. Below 210°C, sucrose does not efficiently transform into furan aldehydes, leading to poor water resistance.

Optimal Parameters

The peak performance was reached with the following configuration:

  • Temperature: 220°C
  • Time: 1.2 min/mm
  • Tannin-to-Sucrose Ratio: 60:40
  • Adhesive Loading: 160 g/m²

At these settings, the wet bonding strength in boiling water reached 0.83 MPa, surpassing the 0.70 MPa requirement for Type-I plywood (GB/T 17657-2013). XRD analysis further supported this, showing maximum molecular crystallinity (33.13%) at 220°C. Interestingly, increasing the temperature to 230°C caused a decline in strength, likely due to the thermal degradation of the wood or the cured adhesive.

Conclusion and Future Directions

While the tannin-sucrose adhesive proves that a 100% biomass solution can meet rigorous industrial standards, the required hot-pressing temperature of 220°C is significantly higher than standard industrial practices (120°C–150°C). This high energy demand is a barrier to commercial adoption.

Future research will focus on identifying catalysts that can lower the activation energy for the sucrose-to-5-HMF transformation. Achieving high-strength bonding at lower temperatures will be the key to making this sustainable adhesive a viable replacement for traditional synthetic resins.

Summary updated

Abstract

Biomass adhesive is conducive to decreasing the dependence of the wood adhesive industry on synthetic resin based on fossil resources and improving the market competitiveness of adhesives. It is also a critical breakthrough to realize the goal of carbon peaking and carbon neutrality in the wood industry. In this study, a full biomass wood adhesive composed of tannin and sucrose was developed and applied successfully to the preparation of plywood. The preparation technique of plywood was optimized, and the chemical structure, curing performance, crystallization property and thermal performance of the adhesive were investigated. Results showed that: (1) hot-pressing temperature played a decisive role in the performances of tannin-sucrose composite adhesives and it also had a very significant influence on the water resistance of plywood. (2) The preparation of tannin-sucrose composite adhesive was a process in which sucrose was transformed into furan aldehydes and then made cross-linking reaction with tannin. These composite adhesives could only get good bonding performances when the curing temperature was above 210°C. (3) The optimal plywood preparation technique was: hot-pressing temperature of 220°C, hot-pressing time of 1.2 min/mm, m(tannin):m(sucrose) of 60:40, and adhesive loading of 160 g/m<sup>2</sup>. The wet bonding strength in boiling water of the prepared plywood was 0.83 MPa, meeting the strength requirements of Type-I plywood in the standard of GB/T 17657-2013. (4) The curing temperature of tannin-sucrose composite adhesive was further decreased by lowering the temperature during the transformation of sucrose into 5-HMF, which was a key in subsequent research.
BibTeX
@article{gu2023study,
  author = {Wen Gu and Xinyue Ding and Min Tang and Feiyan Gong and Shuangshuang Yuan and Jintao Duan},
  title = {{Study on the Preparation Process Optimization of Plywood Based on a Full Biomass Tannin-Sucrose Wood Adhesive}},
  journal = {JOURNAL},
  year = {2023},
  doi = {10.32604/jrm.2023.027461},
}
Figure