Effect of matrix composition on the performance of calcium carbonate filled poly(lactic acid)/poly(butylene adipate- co -terephthalate) composites

Zhenyu Guo, Weiqiang Song, Xueqin Wei, Feng Yu, Yixuan Song, Zidong Guo, Wenxi Cheng, Wei Miao, Bo Cheng, Shiping Songe-Polymers 2023 · DOI

Abstract

The ratio of poly(lactic acid) (PLA), poly(butylene adipate-co-terephthalate) (PBAT), and calcium carbonate ($CaCO_3$) fillers in PLA/PBAT/$CaCO_3$ composites was set at 90/10/5, 70/30/5, and 30/70/5. The effect of nano- and micro-$CaCO_3$ on the melting and crystallization performance of the composites was investigated by differential scanning calorimetry (DSC). PLA crystallization was related to the PLA/PBAT ratio, cooling rate, and $CaCO_3$ particle size. Nano-$CaCO_3$ prevented the crystallization of PLA in PLA-rich blends (90/10 and 70/30) but did not prevent it in PBAT-rich blends (30/70). Unlike nano-$CaCO_3$, micro-$CaCO_3$ did not prevent PLA crystallization regardless of the polymer ratio. Mechanical properties of PBAT-rich composites were significantly improved due to the good compatibility between the $CaCO_3$ filler and PBAT.

Introduction

Biodegradable polymers like PLA are promising alternatives to petroleum-based plastics but suffer from brittleness and high cost. Blending PLA with flexible PBAT improves toughness, but these blends remain expensive. Adding inorganic fillers like calcium carbonate ($CaCO_3$) can lower costs and tune properties. However, the filler's particle size (nano vs. micro) and the polymer matrix ratio significantly influence crystallization and mechanical performance. This study investigates these interactions to optimize "green" materials for applications like agriculture and packaging.

Methods

Composites were prepared with three PLA/PBAT ratios (90/10, 70/30, and 30/70) and 5 parts of either nano-sized or micro-sized $CaCO_3$.

  • Processing: Melt-blending via twin-screw extruder followed by injection molding.
  • Thermal Analysis: DSC was used to study melting and crystallization behavior. Kinetics were modeled using Avrami, Jeziorny, and Mo methods.
  • Mechanical Testing: Tensile and Izod impact tests measured strength and toughness.
  • Morphology: Scanning Electron Microscopy (SEM) examined fracture surfaces.

Thermal Behavior and Crystallization

The thermal properties of the composites are highly dependent on the matrix composition and filler size. DSC analysis revealed that in PLA-rich blends (90/10 and 70/30), nano-$CaCO_3$ inhibits PLA crystallization during cooling. This is attributed to a "nano-confinement" effect where the high surface area of nanoparticles restricts PLA chain mobility, effectively freezing them in an amorphous state.

DSC curves and thermal property data for PLA/PBAT/CaCO3 composites.

The crystallization kinetics were further analyzed using the Mo method, which relates the cooling rate to the crystallization time. The results showed that PBAT crystallization in PBAT-rich (30/70) blends is exceptionally fast, which is critical for industrial high-speed manufacturing processes.

Non-isothermal crystallization kinetics and Mo method parameters.

Mechanical Performance and Morphology

The most significant mechanical improvements were observed in PBAT-rich (PLA30) samples. $CaCO_3$ has a higher affinity for PBAT, leading to better dispersion in the continuous PBAT phase of the 30/70 blend. For the PLA30NC5 sample (PBAT-rich with nano-filler), the elongation at break reached a staggering 764%, with a substantial increase in impact strength. SEM imaging confirmed that in PBAT-rich blends, particles were well-embedded, whereas in PLA-rich blends, they often appeared poorly integrated, explaining the difference in performance gains.

Conclusion

The performance of PLA/PBAT/$CaCO_3$ composites is dictated by the synergy between the polymer ratio and filler size. While nano-$CaCO_3$ can inhibit crystallization in PLA-rich matrices, it serves as an excellent toughening agent in PBAT-rich formulations. These findings provide a roadmap for designing cost-effective, high-performance biodegradable composites by leveraging matrix-filler compatibility.

Summary updated

Abstract

Abstract The ratio of poly(lactic acid) (PLA), poly(butylene adipate- co -terephthalate) (PBAT), and calcium carbonate (CaCO 3 ) fillers in PLA/PBAT/CaCO 3 composites was set at 90/10/5, 70/30/5, and 30/70/5. The effect of nano- and micro-CaCO 3 on the melting and crystallization performance of the composites was investigated by differential scanning calorimetry. PLA crystallization was related to the PLA and PBAT ratio, cooling rate, and CaCO 3 particle size in PLA/PBAT/CaCO 3 composites. Nano-CaCO 3 prevented the crystallization of PLA in PLA/PBAT/CaCO 3 90/10/5 and 70/30/5 but did not prevent the crystallization of PLA in PLA/PBAT/CaCO 3 30/70/5. Unlike nano-CaCO 3 , micro-CaCO 3 did not prevent PLA crystallization regardless of the PLA and PBAT ratio. Nano- and micro-CaCO 3 enhance PLA90 and PLA70 to some extent, due to the aggregation and dissociation of the CaCO 3 filler in polylactic acid. But nano- and micro-CaCO 3 improved the mechanical properties of PLA30 several times, due to the good compatibility of the CaCO 3 filler and PBAT. The effect of nano-CaCO 3 and micro-CaCO 3 on the mechanical properties of PLA/PBAT/CaCO 3 composites had no significant difference.
BibTeX
@inproceedings{guo2023effect,
  author = {Zhenyu Guo and Weiqiang Song and Xueqin Wei and Feng Yu and Yixuan Song and Zidong Guo and Wenxi Cheng and Wei Miao and Bo Cheng and Shiping Song},
  title = {{Effect of matrix composition on the performance of calcium carbonate filled poly(lactic acid)/poly(butylene adipate- <i>co</i> -terephthalate) composites}},
  booktitle = {e-Polymers},
  year = {2023},
  doi = {10.1515/epoly-2023-0026},
}
Figure