Effect of Ce<sub>2</sub>O<sub>3</sub> on Viscosity and Structure for CaO–SiO<sub>2</sub>–Al<sub>2</sub>O<sub>3</sub>-based Mold Flux

Boyang Li, Xin Geng, Zhouhua Jiang, Wei GongISIJ 2022 · DOI

Introduction

In the continuous casting of high-alloy steels, "mold flux" plays a pivotal role as a lubricant and heat transfer controller between the solidifying steel and the water-cooled mold. Traditional fluxes, primarily composed of CaO-SiO₂, face challenges when casting steels with reactive elements like Aluminum (Al). The chemical reaction between Al in the steel and SiO₂ in the flux increases alumina (Al₂O₃) content, leading to undesirable changes in viscosity and crystallization behavior. This study investigates the potential of Cerium oxide (Ce₂O₃) as a modifier to stabilize CaO–SiO₂–Al₂O₃-based fluxes.

Methods and Materials

Researchers prepared five mold flux samples (S0 to S4) with Ce₂O₃ mass percentages ranging from 0% to 20%. The base composition was fixed at 30%CaO-30%SiO₂-15%Al₂O₃-5%MgO-10%Na₂O-10%CaF₂. The viscosity was measured using the rotating column method across a range of temperatures. Structural analysis was conducted using Raman spectroscopy and X-ray diffraction (XRD) to understand the atomic-scale changes and crystalline phases formed during cooling.

Results and Discussion

Impact on Viscosity and Melt Structure

The addition of Ce₂O₃ significantly influences the fluid properties of the mold flux. At high temperatures (above 1670 K), increasing Ce₂O₃ content leads to a noticeable decrease in viscosity. This is attributed to Ce₂O₃ acting as a "network breaker." Upon dissociation into Ce³⁺ and O²⁻ ions, the free oxygen attacks the silicate network, breaking complex silica tetrahedra chains into simpler, smaller units. This structural simplification reduces internal friction during flow.

Viscosity vs. temperature curves for mold flux samples with varying Ce2O3 content.

Raman spectroscopy confirmed this trend, showing a shift in peaks that indicates a lower degree of polymerization (NBO/T values increased from 2.02 to 2.18). Interestingly, while the silicate network is heavily modified, the aluminate structure remains largely unaffected, suggesting a selective interaction.

Crystallization and the Break Temperature Paradox

While Ce₂O₃ improves fluidity at high temperatures, it also enhances the crystallization ability of the flux. As the temperature drops, the primary crystalline phase shifts from cuspidine (Ca₄Si₂O₂F) to cerium silicate (Ce₉.₃₃(SiO₄)₆O₂). This shift leads to an increase in the "break temperature" (T_br), the point where the flux transitions from a liquid-like state to a solid-like state.

Arrhenius plots of ln(viscosity) vs. 1/T, highlighting the increase in break temperature (Tbr) with Ce2O3 addition.

As shown in the Arrhenius plots, the T_br rises from 1418 K for the base sample (S0) to 1507 K for the 20% Ce₂O₃ sample (S4). This increase in T_br is a critical factor for industrial application, as an excessively high break temperature can lead to a thin liquid film and poor lubrication, potentially causing surface defects or breakouts.

Conclusion

The study demonstrates that Ce₂O₃ is an effective modifier for CaO–SiO₂–Al₂O₃-based mold fluxes, improving high-temperature fluidity by simplifying the silicate network. However, due to the significant increase in crystallization temperature, the researchers recommend that Ce₂O₃ content should not exceed 15% by mass to maintain optimal lubrication and heat transfer during the continuous casting process.

Summary updated

Abstract

The viscosity of 30%CaO-30%SiO2-15%Al2O3-5%MgO-10%Na2O-10%CaF2-xCe2O3 (mass%, x = 0, 5, 10, 15) were measured by the rotating column method, and then the viscosity and the Tbr (break temperature) of the mold flux were analyzed based on the results. Meanwhile, the structural characteristics of the mold flux were investigated using Raman spectroscopy and XRD (X-ray diffraction). The results show that Ce2O3 predominantly destroys the silicate network structure at high temperature, reduces the polymerization degree of the mold flux, simplifies the high-temperature structure of the mold flux, and reduces the friction resistance of viscous flow. From the apparent phenomenon, the viscosity of the mold flux decreases at high temperature. In addition, with the increase of Ce2O3 content in the mold flux, Ca4Si2O2F changes to Ce9.33(SiO4)6O2, which enhances the crystallization ability of the mold flux and increases the Tbr of the mold flux.
BibTeX
@inproceedings{li2022effect,
  author = {Boyang Li and Xin Geng and Zhouhua Jiang and Wei Gong},
  title = {{Effect of Ce\<sub\>2\</sub\>O\<sub\>3\</sub\> on Viscosity and Structure for CaO–SiO\<sub\>2\</sub\>–Al\<sub\>2\</sub\>O\<sub\>3\</sub\>-based Mold Flux}},
  booktitle = {ISIJ},
  year = {2022},
  doi = {10.2355/isijinternational.isijint-2021-554},
}
Figure