Effect of a Small Amount of Hydrogen on Cyclic Shape Memory Behavior of Ti-Ni Alloy

Teruo Asaoka, Taisuke Kamimura, Hideo Saitô, Yōichi IshidaJournal of the Japan Institute of Metals and Materials 1992 · DOI

Abstract

The effect of hydrogen on the cyclic shape memory behavior of Ti-Ni alloy has been studied. A cyclic test machine was constructed. As the result, shape memory recovery stress and recovery % decreased with a small amout of hydrogen absorption. After degasing of the hydrogen following the cathodic charge, recovery stress and recovery % approached the level of a hydrogen-free specimen. The rate of this approaching depended on the amount of cyclic strains. During deformations at martensitic phases, no effect of hydrogen was observed on the coalescence of martensite variants. The decrease in recovery stress under mild hydrogen conditions, in which no hydride has been formed, was attributed to interactions between mobile hydrogen and dislocation introduced by the cyclic deformations.

Introduction

Titanium-Nickel (Ti-Ni) alloys are the "gold standard" for shape memory applications, utilized in critical components such as medical stents and actuators. While the effects of major impurities like oxygen and carbon are well-documented, the impact of trace hydrogen—absorbed during manufacturing processes like acid pickling or during service in corrosive environments—remains under-studied. This research investigates how microscopic amounts of hydrogen, insufficient to form brittle hydrides, affect the alloy's ability to perform repeatedly over hundreds of cycles.

Experimental Methods

The study utilized Ti-50.0 at.% Ni wires (1mm diameter) heat-treated at 673K to maintain a high dislocation density, optimizing shape memory performance. To characterize cyclic behavior, the researchers developed a specialized automated testing machine capable of rapid thermal cycling through direct electrical heating and forced-air cooling.

Hydrogen was introduced into the specimens via cathodic charging in a NaOH solution at low current densities (1–5 A/m²). The experimental protocol included degassing tests, where samples were left at room temperature to observe the restoration of mechanical properties as hydrogen diffused out. Mechanical response was evaluated through stress-strain hysteresis loops and recovery stress measurements over up to 1,000 cycles.

Results and Discussion

The introduction of even small amounts of hydrogen led to an immediate decrease in both recovery stress and recovery percentage.

Stress-strain hysteresis loops showing the evolution of cyclic behavior for (a) hydrogen-free and (b) hydrogen-charged specimens.

As illustrated in Figure 4, the stress-strain loops evolve over successive cycles (N=1, 2, 3). In hydrogen-charged specimens, the recovery stress is notably lower compared to hydrogen-free controls. Interestingly, the "plateau" region of the deformation curve, which corresponds to the reorientation of martensite variants, showed no significant change. This suggests that hydrogen does not hinder the phase-change mechanism itself but instead interacts with the dislocation network introduced by cyclic deformation.

The severity of this degradation is highly sensitive to the magnitude of the cyclic strain. At a 2% cyclic strain, the material remains relatively stable, with degradation typically plateauing within the first 100 cycles. However, at higher strains of 3–4%, hydrogen significantly accelerates fatigue and plastic deformation.

Accumulation of plastic elongation over 1,000 cycles at various strain levels (2%, 3%, and 4%).

Figure 6 demonstrates the accumulation of plastic elongation ($Δl$) over 1,000 cycles. Specimens subjected to 4% strain exhibit a rapid and substantial increase in plastic elongation, whereas those at 2% strain remain comparatively stable. This supports the hypothesis that hydrogen interacts with mobile dislocations, which are generated more prolifically at higher strain levels.

A critical finding of this study is the reversibility of the hydrogen effect. Because no stable hydrides are formed at these low concentrations, the "poisoning" of the shape memory effect is temporary. Degassing the specimens for approximately 22 hours allowed the recovery stress to return to nearly original levels, confirming that the interaction is transient.

Conclusion

For high-reliability applications, engineers must account for hydrogen absorption, particularly in components undergoing high-strain cycles in corrosive or biological environments. The study concludes that hydrogen reduces the apparent energy available for shape recovery by interfering with internal stress fields and dislocation movement. Managing hydrogen exposure is essential to maintaining the cyclic stability and longevity of Ti-Ni shape memory alloys.

Summary updated

Abstract

The effect of hydrogen on the cyclic shape memory behavior of Ti-Ni alloy has been studied. A cyclic test machine was constructed. As the result, shape memory recovery stress and recovery % decreased with a small amout of hydrogen absorption. After degasing of the hydrogen following the cathodic charge, recovery stress and recovery % approached the level of a hydrogen-free specimen. The rate of this approaching depended on the amount of cyclic strains. During deformations at martensitic phases, no effect of hydrogen was observed on the coalescence of martensite variants. The decrease in recovery stress under mild hydrogen conditions, in which no hydride has been formed, was attributed to interactions between mobile hydrogen and dislocation introduced by the cyclic deformations.
BibTeX
@article{asaoka1992effect,
  author = {Teruo Asaoka and Taisuke Kamimura and Hideo Saitô and Yōichi Ishida},
  title = {{Effect of a Small Amount of Hydrogen on Cyclic Shape Memory Behavior of Ti-Ni Alloy}},
  journal = {Journal of the Japan Institute of Metals and Materials},
  year = {1992},
  doi = {10.2320/jinstmet1952.56.10\_1111},
}
Figure