Effect of a Small Amount of Hydrogen on the Pseudo-Elastic Properties of Ti-Ni Alloy

Teruo Asaoka, Hideaki Yamashita, Hideo Saitô, Yōichi IshidaJournal of the Japan Institute of Metals and Materials 1993 · DOI

Abstract

The effect of a small amount of hydrogen on the cyclic pseudo-elastic properties of a Ti-Ni alloy has been studied. A cyclic test machine and control systems were constructed for the study. A decrease in the pseudo-elastic properties due to the absorption of a small amount of hydrogen was observed. Hydrogen seems to reduce or shift the stress-temperature range for the appearance of pseudo-elasticity. The changes in pseudo-elastic properties during the cyclic test were attributed to the accumulation of plastic strain at local regions such as grain boundaries and hydrogen induced decrease in the critical stress for slip deformation. Hydrogen is thought to have an interaction with dislocations and lead to the local formation of stress induced martensites. Dissolved or trapped hydrogen, or both, are supposed to have played an important role during the processes.

Introduction

Titanium-Nickel (Ti-Ni) alloys, commonly known as Nitinol, are celebrated for their "superelasticity" (or pseudo-elasticity)—the ability to undergo large deformations and return to their original shape upon unloading. This unique property makes them ideal for critical applications in medical implants, aerospace components, and nuclear environments. However, these environments often expose the alloy to hydrogen (e.g., from biological fluids or seawater). While previous research has explored hydrogen's impact on the shape memory effect, there has been a significant gap in understanding its effect on cyclic superelasticity—specifically how the material performs over thousands of loading cycles in hydrogen-rich conditions. This study quantifies this degradation and investigates the underlying microstructural mechanisms.

Methods

The researchers utilized a Ti-50.0 at% Ni wire (1mm diameter), annealed to retain a high dislocation density, which is known to optimize superelastic performance.

  • Hydrogen Charging: Hydrogen was introduced using a cathodic electrolytic charging method in a NaOH solution. By varying the current density (1–5 A/m²), the team achieved estimated hydrogen concentrations of 30–50 ppm.
  • Custom Testing Rig: Because superelasticity is highly temperature-dependent, a specialized cyclic testing machine was constructed. It employed a direct-current heating system and PID control to maintain the sample at a constant 353 K, well above the austenite finish temperature ($A_f$).
  • Cyclic Loading: Samples were subjected to 1,000 cycles of 2–4% strain.
  • Analysis: The team measured transformation temperatures via Differential Scanning Calorimetry (DSC), analyzed stress-strain hysteresis loops to calculate energy dissipation, and used Scanning Electron Microscopy (SEM) to inspect fracture surfaces.

Results and Discussion

A primary observation during the cyclic tests was the "thinning" of the superelastic hysteresis loop as cycles progressed. This phenomenon indicates a reduction in the energy dissipated per cycle and a shift in the material's transformation behavior. Hydrogen was found to significantly accelerate this process.

Evolution of stress-strain hysteresis loops and temperature stability during cyclic testing.

The study identified that hydrogen interacts with dislocations to lower the apparent critical stress required for slip deformation. Essentially, hydrogen makes it easier for the metal to undergo permanent plastic deformation rather than reversible elastic transformation. This is quantified by the parameter $E_s$ (the ratio of elastic recovery), which drops more sharply in hydrogen-charged samples, particularly within the first 200 cycles.

Quantitative degradation of superelastic properties (stress $\sigma_s$ and recovery ratio $E_s$) over 1,000 cycles.

Furthermore, hydrogen tends to accumulate at grain boundaries and defects, promoting the localized formation of "stress-induced martensite" that becomes trapped and does not revert to austenite upon unloading. This accumulation of "dead" martensite at local regions eventually leads to crack initiation. While hydrogen-free samples typically cleared 1,000 cycles without issue, samples charged at higher current densities (4–5 A/m²) saw their fatigue life collapse to fewer than 50 cycles. Interestingly, SEM images showed "dimple" patterns on fracture surfaces, suggesting that despite the early failure, the microscopic break was ductile, driven by localized plastic strain.

Conclusion and Future Work

Trace amounts of hydrogen (30–50 ppm) significantly degrade the cyclic superelastic performance of Ti-Ni alloys by lowering the barrier for slip deformation and promoting localized martensite trapping.

Limitations of the current study include the estimation of hydrogen levels based on charging conditions rather than direct measurement of every sample. Future research should investigate how different heat treatments might mitigate these effects by altering dislocation structures. Additionally, studying these effects at varying strain rates could clarify if hydrogen diffusion speed is a limiting factor in cyclic degradation.

Summary updated

Abstract

The effect of a small amount of hydrogen on the cyclic pseudo-elastic properties of a Ti-Ni alloy has been studied. A cyclic test machine and control systems were constructed for the study. A decrease in the pseudo-elastic properties due to the absorption of a small amount of hydrogen was observed. Hydrogen seems to reduce or shift the stress-temperature range for the appearance of pseudo-elasticity. The changes in pseudo-elastic properties during the cyclic test were attributed to the accumulation of plastic strain at local regions such as grain boundaries and hydrogen induced decrease in the critical stress for slip deformation. Hydrogen is thought to have an interaction with dislocations and lead to the local formation of stress induced martensites. Dissolved or trapped hydrogen, or both, are supposed to have played an important role during the processes.
BibTeX
@article{asaoka1993effect,
  author = {Teruo Asaoka and Hideaki Yamashita and Hideo Saitô and Yōichi Ishida},
  title = {{Effect of a Small Amount of Hydrogen on the Pseudo-Elastic Properties of Ti-Ni Alloy}},
  journal = {Journal of the Japan Institute of Metals and Materials},
  year = {1993},
  doi = {10.2320/jinstmet1952.57.10\_1123},
}
Figure