Upcycling of Waste PVC into CaCO3/KOH-Modified Porous Carbon for Supercapacitor Applications

Wenbo Cai, Le Liu, Peng Zhang, Zhidan LinMolecules 2025 · DOI

TL;DR

This paper presents a novel, eco-friendly method to transform waste PVC plastic into high-performance porous carbon materials for supercapacitors. By employing a two-step activation process using calcium carbonate and potassium hydroxide, they created a hierarchical porous structure with excellent electrochemical properties, demonstrating a promising route for both waste management and energy storage.

What Problem Does This Paper Address?

The ever-increasing demand for energy storage devices, particularly supercapacitors (SCs), is driving the need for advanced electrode materials. While porous carbons are ideal candidates due to their cost-effectiveness and stability, their widespread commercialization is hampered by limitations in energy density and specific capacitance. Furthermore, the growing problem of plastic waste, specifically polyvinyl chloride (PVC), poses significant environmental challenges. Traditional methods for recycling PVC are often inefficient and can lead to further pollution. This paper tackles both issues by proposing a method to upcycle waste PVC into high-value porous carbon materials suitable for supercapacitor applications, addressing the dual need for sustainable waste management and improved energy storage solutions.

Methods

The researchers developed a two-step activation strategy for porous carbon synthesis from PVC.

  1. CaCO<sub>3</sub> Pre-activation: Waste PVC was blended with calcium carbonate (CaCO<sub>3</sub>) and heated under a nitrogen atmosphere. This step serves multiple purposes:
  2. HCl Capture: During PVC pyrolysis, HCl gas is released. CaCO<sub>3</sub> reacts with HCl, forming CaCl<sub>2</sub> and water, thus mitigating equipment corrosion.
  3. Mesopore Formation: The decomposition of CaCO<sub>3</sub> releases CO<sub>2</sub>, which acts as a gas-phase activator, etching the carbon to form mesopores.
  4. Sacrificial Template: Nano-CaO particles formed from CaCO<sub>3</sub> decomposition act as sacrificial templates, contributing to pore structure development.
  5. Acid Washing: After pyrolysis, the material was treated with HCl to remove CaCO<sub>3</sub> by-products, further shaping the porous framework.
  6. KOH Activation: The resulting carbon material was then subjected to secondary activation with potassium hydroxide (KOH) at varying ratios (C-PVC:KOH = 1:1 to 1:3). This step is crucial for:
  7. Micropore Development: KOH acts as a chemical activator, etching the carbon to create a high density of micropores.
  8. Oxygen Doping: The activation process also introduces oxygen-containing functional groups onto the carbon surface.

The synthesized materials were characterized using Scanning Electron Microscopy (SEM), Transmission Electron Microscopy (TEM), X-ray Diffraction (XRD), X-ray Photoelectron Spectroscopy (XPS), Fourier Transform Infrared Spectroscopy (FTIR), and Brunauer-Emmett-Teller (BET) analysis for surface area and pore size distribution. Electrochemical performance was evaluated using cyclic voltammetry (CV), galvanostatic charge-discharge (GCD), and electrochemical impedance spectroscopy (EIS).

Datasets

Not discussed in the paper. The study focuses on material synthesis and characterization, with electrochemical testing performed on the synthesized materials.

Key Insights and Ideas

  • Synergistic Activation: The combination of CaCO<sub>3</sub> and KOH activation is key. CaCO<sub>3</sub> handles the corrosive HCl and creates mesopores, while KOH fine-tunes the microporosity and enhances surface area. This dual approach is more effective than single-step activation.
  • Waste Upcycling: Successfully transforming problematic PVC waste into a valuable material for energy storage highlights a significant step towards a circular economy.
  • Oxygen Doping Benefits: The introduction of oxygen-containing functional groups (C-O, C=O) significantly improves the material's wettability and electrochemical performance by enhancing pseudocapacitance and facilitating electrolyte penetration.
  • Optimal KOH Ratio: There's a sweet spot for KOH activation. Too little, and the microporosity isn't fully developed; too much leads to over-activation, pore collapse, and reduced surface area. The 1:2 ratio (C-KOH-2) proved optimal.
  • Hierarchical Porosity is Crucial: The combination of micropores (for high surface area and charge storage) and mesopores (for efficient ion transport) is essential for achieving high specific capacitance and rate capability.

Key Results

  • Optimal Material (C-KOH-2): The C-KOH-2 sample, prepared with a C-PVC:KOH ratio of 1:2, exhibited the best performance.
  • High Specific Surface Area: Achieved a specific surface area of 1729 m²/g.
  • Oxygen Doping: The optimal material contained 7.37% oxygen doping.
  • High Specific Capacitance: C-KOH-2 delivered a specific capacitance of 360.4 F/g at 1 A/g.
  • Excellent Rate Capability: Retained 72.1% of its capacitance at a high current density of 10 A/g.
  • Supercapacitor Performance: Symmetric supercapacitors fabricated with C-KOH-2 electrodes achieved an energy density of 9.9 Wh/kg at 125 W/kg.
  • Exceptional Cycling Stability: The supercapacitors maintained 93.12% of their initial capacitance after 5000 charge-discharge cycles at 1 A/g.
  • Improved Wettability: The oxygen-doped C-KOH-2 showed a significantly lower contact angle (115.4°) compared to commercial activated carbon (145.1°), indicating enhanced hydrophilicity.

Limitations and Future Work

  • Limitations:
    • The paper focuses on the electrochemical performance of the electrode material itself. While a symmetric supercapacitor was built and tested, further optimization of the entire device (electrolyte, separator, cell design) could potentially yield even better results.
  • The study mentions the use of plasticizers and thermal stabilizers in PVC, which can complicate recycling. While the CaCO<sub>3</sub> method addresses chlorine, the impact of other additives on the final carbon material's properties might warrant further investigation.
  • Future Work:
    • The authors suggest that this dual-purpose approach can be extended to other plastic wastes.
  • Further exploration of different activation ratios and conditions could lead to even more optimized porous carbon structures.
  • Investigating the long-term stability and performance under more demanding real-world conditions would be beneficial.
  • The paper demonstrated powering a blue LED, suggesting potential applications in flexible electronics and emergency power supplies, which could be a focus for future development.

Summary updated

Abstract

This study introduces a green method for converting waste polyvinyl chloride (PVC) into hierarchical porous carbon materials. By using CaCO<sub>3</sub> pre-activation to capture HCl and form meso/macroporous frameworks, followed by KOH activation to tune microporosity, high-surface-area porous carbon was successfully produced. The effects of KOH loading ratios (C-PVC:KOH = 1:1 to 1:3) on the primary activated carbon material were systematically investigated. It was found that a ratio of 1:2 (C-KOH-2) yielded optimal material properties, with a specific surface area of 1729 m<sup>2</sup> g<sup>-1</sup> and an oxygen doping content of 7.37%. Electrochemical measurements revealed that C-KOH-2 exhibited a high specific capacitance of 360.4 F g<sup>-1</sup> at 1 A g<sup>-1</sup>, retaining 72.1% of its capacitance at 10 A g<sup>-1</sup>. The symmetric supercapacitors achieved an energy density of 9.9 Wh kg<sup>-1</sup> at 125 W kg<sup>-1</sup>, with 93.12% capacitance retention over 5000 cycles. This dual-purpose approach enables the upcycling of PVC waste while promoting the development of high-performance electrodes.
BibTeX
@inproceedings{cai2025upcycling,
  author = {Wenbo Cai and Le Liu and Peng Zhang and Zhidan Lin},
  title = {{Upcycling of Waste PVC into CaCO3/KOH-Modified Porous Carbon for Supercapacitor Applications}},
  booktitle = {Molecules},
  year = {2025},
  doi = {10.3390/molecules30163420},
}
Figure