Sintering and Rolling Behavior of Cu-50In-13Ga Ternary Alloy Powder for Sputtering Target

Dae‐Won Kim, Yong‐Ho Kim, Jung‐Han Kim, Jong‐Hyeon Lee, Kwang-Bo Choi, Hyeon‐Taek SonJournal of Korean Powder Metallurgy Institute 2012 · DOI

Abstract: In this study, we mainly focus on the study of densification of gas-atomized Cu-50 wt.%In-13 wt.%Ga alloy powder without occurrence of crack during the forming process. Cu-50 wt.%In-13 wt.%Ga alloy powder was consolidated by sintering and rolling processes in order to obtain high density. The phase and microstructure of formed materials were examined by X-ray diffraction (XRD), scanning electron microscopy (SEM) and optical microscopy (OM), respectively. Warm rolling using copper can result in the improvement of density. The specimen obtained with 80% of rolling reduction ratio at $140^{\circ}C$ using cooper can have the highest density of $8.039g/cm^3$.

Introduction

Copper Indium Gallium Selenide (CIGS) thin-film solar cells are highly regarded for their efficiency and stability. However, the quality of these films is intrinsically linked to the sputtering targets used in their production. Porous targets often lead to "arcing"—electrical discharges that release unwanted particles and gases, causing defects in the solar cell and reducing energy conversion efficiency. Achieving near-theoretical density in these targets is therefore a critical manufacturing goal.

Experimental Methods

The researchers utilized gas-atomized Cu-50wt.%In-13wt.%Ga powder as the starting material. The primary challenge in consolidating this alloy is the low melting point of Indium (~156°C). To understand the thermal behavior and determine optimal processing windows, Differential Scanning Calorimetry (DSC) was employed.

Heat flow analysis identifying the melting point of Indium (P1) at approximately 156°C.

Two consolidation paths were compared:

  1. Conventional Sintering & Rolling: Powders were pressed and sintered at temperatures between 300°C and 500°C, followed by hot rolling.
  2. Canning Rolling: Raw powder was packed into a pure copper "can" and "warm rolled" at 140°C—strategically chosen to be just below the melting point of indium to maintain its solid state while utilizing its softness for mechanical densification.

Results and Discussion

The Sintering Paradox

Conventional sintering at 500°C achieved a density of approximately 7.8 g/cm³. However, this high-temperature process caused significant indium exudation (bleeding), which left behind needle-like pores at grain boundaries. Interestingly, subsequent rolling of these sintered samples actually decreased their density, as the mechanical strain caused these pores to expand rather than close.

Density trends as a function of sintering temperature and physical appearance of the resulting compacts.

The Canning Advantage

The novel canning rolling approach at 140°C bypassed the issues of liquid-phase migration. By applying high hydrostatic pressure while the indium remained solid, the researchers achieved a maximum density of 8.039 g/cm³, representing 99.7% of the theoretical density. Microstructural analysis confirmed that this method eliminated internal voids and produced a highly integrated bulk material without the cracks typical of conventional processing.

Conclusion

This research demonstrates that low-temperature canning rolling is a superior method for producing high-density Cu-In-Ga sputtering targets. By operating just below the melting point of indium, manufacturers can achieve near-theoretical density and avoid the microstructural defects associated with high-temperature sintering. Future studies should evaluate the sputtering performance and arcing frequency of these ultra-dense targets in vacuum deposition environments.

Summary updated

Abstract

In this study, we mainly focus on the study of densification of gas-atomized Cu-50 wt.%In-13 wt.%Ga alloy powder without occurrence of crack during the forming process. Cu-50 wt.%In-13 wt.%Ga alloy powder was consolidated by sintering and rolling processes in order to obtain high density. The phase and microstructure of formed materials were examined by X-ray diffraction (XRD), scanning electron microscopy (SEM) and optical microscopy (OM), respectively. Warm rolling using copper can result in the improvement of density. The specimen obtained with 80% of rolling reduction ratio at <TEX>$140^{\circ}C$</TEX> using cooper can have the highest density of <TEX>$8.039g/cm^3$</TEX>.
BibTeX
@article{kim2012sintering,
  author = {Dae‐Won Kim and Yong‐Ho Kim and Jung‐Han Kim and Dae Geun Kim and Jong‐Hyeon Lee and Kwang-Bo Choi and Hyeon‐Taek Son},
  title = {{Sintering and Rolling Behavior of Cu-50In-13Ga Ternary Alloy Powder for Sputtering Target}},
  journal = {Journal of Korean Powder Metallurgy Institute},
  year = {2012},
  doi = {10.4150/kpmi.2012.19.4.264},
}
Figure