Reversibility of Al/Ti Modified LiBH4

Didier Blanchard, Qing Shi, Chris Boothroyd, Tejs VeggeThe Journal of Physical Chemistry C 2009 · DOI

TL;DR

This paper investigates modifying lithium borohydride (LiBH<sub>4</sub>) with aluminum (Al) and titanium (Ti) compounds to improve its hydrogen storage capabilities for mobile applications. They found that Al, particularly when combined with Ti in an Al-Ti solid solution, significantly lowers the temperature and pressure required for hydrogen release and uptake, while also enhancing the reversibility of the process.

What Problem Does This Paper Address?

Storing hydrogen efficiently and safely for mobile applications, such as in fuel cell vehicles, is a major challenge. Lithium borohydride (LiBH<sub>4</sub>) is a promising material due to its high gravimetric hydrogen capacity (18.5 wt%). However, its practical use is hindered by the high temperatures and pressures required for its hydrogenation and dehydrogenation cycles. Pure LiBH<sub>4</sub> decomposes at temperatures above 380 °C, and achieving full reversibility requires even more extreme conditions. This paper aims to address this by exploring how modifying LiBH<sub>4</sub> with additives, specifically aluminum and titanium compounds, can lower these operating conditions and improve the kinetics and reversibility of hydrogen storage.

Methods

The researchers employed several key techniques:

  • Ball Milling: This high-energy mechanical process was used to mix LiBH<sub>4</sub> with various aluminum and titanium sources (primarily lithium alanate, LiAlH<sub>4</sub>, and titanium trichloride, TiCl<sub>3</sub>). This method is crucial for creating intimate contact and potentially inducing reactions between the components.
  • Thermal Desorption Spectroscopy (TDS): This technique was used to measure the amount of hydrogen released from the samples as a function of temperature. It helps determine the decomposition temperatures and the total hydrogen capacity.
  • Powder X-ray Diffraction (PXD): PXD was used to identify the crystalline phases present in the samples before and after milling, as well as after hydrogen cycling. This allowed the researchers to understand the chemical transformations occurring.
  • Transmission Electron Microscopy (TEM) and Electron Energy Loss Spectroscopy (EELS): These advanced microscopy techniques were used to examine the microstructure of the modified materials, including the size and morphology of crystallites and the elemental composition of specific regions.
  • Quantitative Phase Analysis (QPA): This method, often performed in conjunction with PXD, quantifies the relative amounts of different crystalline phases in a sample.

Datasets

Not discussed in the paper. The study focuses on experimental synthesis and characterization of modified LiBH<sub>4</sub> materials.

Key Insights and Ideas

  • Synergistic Effect of Al and Ti: While Al alone shows activity in lowering decomposition temperatures, its effect is significantly enhanced when combined with Ti, particularly in the form of an Al-Ti solid solution (ss). This suggests a cooperative mechanism at play.
  • Role of LiAlH<sub>4</sub>: Lithium alanate (LiAlH<sub>4</sub>) acts as a convenient source of Al. Its decomposition during milling or heating contributes to the formation of Al and LiH, which are key to modifying LiBH<sub>4</sub>'s properties.
  • Formation of AlB<sub>2</sub>: During the dehydrogenation (hydrogen release) cycle, aluminum diboride (AlB<sub>2</sub>) is formed. Its subsequent disappearance during rehydrogenation (hydrogen uptake) is a hallmark of the reversible cycling process and is linked to improved stability and lower desorption temperatures.
  • Microstructure Matters: TEM analysis revealed that the modified materials consist of Al and/or Al-Ti ss crystallites (around 100 nm) embedded in a porous amorphous matrix. This nanostructure likely plays a crucial role in the enhanced kinetics.
  • Ti's Role in Slow Release: The presence of Ti appears to facilitate a slow release of hydrogen at lower temperatures (around 200 °C), which could be beneficial for certain applications.

Key Results

  • Lowered Decomposition Temperature: Modified LiBH<sub>4</sub> samples decomposed starting at around 200 °C, significantly lower than pure LiBH<sub>4</sub> (above 380 °C).
  • Reversibility at Moderate Conditions: Several samples demonstrated reversibility at approximately 85 bar of H<sub>2</sub> and 350 °C, conditions considered more moderate than those required for pure LiBH<sub>4</sub>.
  • Hydrogen Capacity: The reversible hydrogen capacity was observed to be around 2-2.4 wt% for the entire system, with some samples reaching up to 12-13.5 wt% if considering only the LiBH<sub>4</sub> component.
  • Fast Rehydrogenation: Rehydrogenation was completed within 1-2 hours for some of the reversible samples.
  • Cycling Stability: While reversible, the hydrogen storage capacity decreased with cycling. This loss was attributed to potential B<sub>2</sub>H<sub>6</sub> formation at lower temperatures.

Limitations and Future Work

  • Capacity Loss: The gradual loss of reversible hydrogen storage capacity with cycling is a significant limitation. The authors suggest this might be due to the formation of diborane (B<sub>2</sub>H<sub>6</sub>) at temperatures below 300 °C.
  • Extreme Conditions for Full System: While improved, the conditions (85 bar, 350 °C) are still considered too extreme for widespread mobile applications. The overall system's reversible capacity is also relatively low.
  • Unidentified Peaks: Weak, unidentified peaks were observed in the PXD patterns of cycled samples, suggesting the potential formation of other phases that could contribute to capacity loss.
  • Future Work Suggestions:
    • Investigate methods to avoid B<sub>2</sub>H<sub>6</sub> formation, possibly by using a back-pressure during dehydrogenation.
  • Further studies on the effect of back-pressure during desorption to optimize the formation of AlB<sub>2</sub> and minimize boron segregation.
  • Clarify the nature of the unidentified peaks observed during cycling.
  • Explore other additives or combinations to further improve reversibility and capacity.

Summary updated

Abstract

Lithium borohydride has a high reversible hydrogen storage capacity. For its practical use as an on-board hydrogen storage medium in mobile applications, the temperature and pressure conditions along with the kinetics of the hydrogenation/dehydrogenation cycles have to be improved. Lithium borohydride can be modified by ball-milling with Al- and/or Ti-containing compounds. In this study, lithium alanate (LiAlH4), is used as an Al source. From careful examination of the ball-milled samples, it appears that LiBH4 remains unchanged during milling. The samples contain ∼100 nm diameter Al and/or Al−Ti solid solution (ss) crystallites. When used alone, Ti has a limited effect whereas Al is shown to be active, lowering the temperature of decomposition and increasing the desorption rate and reversibility at moderate temperature and pressure (85 bar, 350 °C). During cycling, AlB2 is formed in the dehydrogenated state and disappears in the hydrogenated state; its formation increases the stability of the products and thus results in a lower desorption temperature. The Al−Ti (ss) also allows a slow release of hydrogen at very low temperatures (200 °C).
BibTeX
@article{blanchard2009reversibility,
  author = {Didier Blanchard and Qing Shi and Chris Boothroyd and Tejs Vegge},
  title = {{Reversibility of Al/Ti Modified LiBH<sub>4</sub>}},
  journal = {The Journal of Physical Chemistry C},
  year = {2009},
  doi = {10.1021/jp9031892},
}
Figure