Research on Fe Removal, Regeneration Process, and Mechanical Properties of Mg Alloy AM50A

Chen Zhao, Zhou Changfa, Wenbo Liu, Sanxing Chen, Gao Cong, Shaowei Jia, Xiaowen Yu, Zhou Wang, Bolin Luo, Qingshuang ZhangCrystals 2024 · DOI

TL;DR

This paper presents an optimized process for removing iron impurities from recycled AM50A magnesium alloy waste, achieving a 96.2% iron removal rate. The regenerated alloy not only matches the original composition but also exhibits significantly improved mechanical properties, including a substantial increase in tensile strength and elongation, making it a viable option for high-performance applications.

What Problem Does This Paper Address?

Magnesium alloys are highly desirable for their lightweight properties, finding widespread use in automotive and electronics industries. However, the increasing application of these alloys generates substantial amounts of waste. This waste often contains impurities, particularly iron, which significantly degrade the mechanical performance and corrosion resistance of the alloy, hindering effective recycling. Current recycling methods for Mg alloys, such as smelting, need efficient ways to remove these detrimental impurities to restore or even enhance the alloy's properties, thereby promoting a circular economy and reducing the environmental impact of primary production.

Methods

The researchers employed a systematic, single-factor experimental approach to identify the optimal conditions for iron removal from AM50A Mg alloy waste. They investigated the influence of three key parameters:

  • Refining Temperature: Experiments were conducted at temperatures ranging from 630 °C to 720 °C to find the optimal temperature for iron removal.
  • Refining Time: The duration of the refining process was varied from 10 to 50 minutes at the optimal temperature to determine the most effective treatment time.
  • Refining Agent Dosage: The mass ratio of the RJ-2 refining agent (a mixture of MgCl₂, KCl, BaCl₂, and NaCl) was tested at levels from 1% to 3% to find the optimal concentration.

After identifying the optimal refining parameters (670 °C, 1.5% RJ-2 agent, 40 min), the regenerated alloy (J40-1.5-AM50A) was characterized using:

  • Inductively Coupled Plasma Emission Spectrometry (ICP): To analyze the elemental composition and confirm iron removal.
  • X-ray Powder Diffraction (XRD): To examine the crystal structure and identify any phase changes or remaining iron compounds.
  • Scanning Electron Microscopy (SEM) and Energy Dispersive X-ray Spectroscopy (EDS): To analyze the surface morphology and elemental distribution, providing visual confirmation of impurity removal.
  • Mechanical Testing: Tensile strength, maximum tensile force, and elongation after fracture were measured to assess the mechanical properties of the original, iron-doped, and regenerated alloys.

Datasets

Not discussed in the paper. The study utilized laboratory-prepared samples of AM50A Mg alloy waste, intentionally doped with iron powder to simulate real-world contaminated waste.

Key Insights and Ideas

  • Iron as a Major Performance Detractor: The study clearly demonstrates that even small amounts of iron significantly degrade the mechanical properties of AM50A magnesium alloy.
  • Optimized Refining is Key: The research highlights that a carefully controlled refining process, rather than just any smelting method, is crucial for effective impurity removal and property restoration.
  • RJ-2 Agent's Dual Role: The RJ-2 refining agent not only facilitates iron removal but also appears to contribute to the improved mechanical properties of the regenerated alloy.
  • Fe Removal Mechanism: The study suggests that iron is removed through deposition, as evidenced by the absence of iron phases in the XRD and EDS analyses of the refined alloy.
  • Regenerated Alloy Outperforms Original: The most striking insight is that the optimized refining process not only removes iron but also results in a regenerated AM50A alloy with superior mechanical properties compared to the original, pristine AM50A.

Key Results

  • Optimal Refining Conditions: The study identified the optimal conditions for iron removal as a refining temperature of 670 °C, a refining agent (RJ-2) mass ratio of 1.5%, and a refining time of 40 minutes.
  • High Iron Removal Rate: Under these optimal conditions, an impressive iron removal rate of 96.2% was achieved.
  • Compositional Consistency: The regenerated J40-1.5-AM50A alloy's composition was found to be consistent with the standard AM50A alloy, with other elemental proportions remaining within acceptable ranges.
  • Significant Mechanical Property Improvement:
    • Compared to the original AM50A sample, the regenerated J40-1.5-AM50A showed a maximum tensile strength increase of 1.611 KN (19.97%) and a tensile strength increase of 26.333 MPa (20.79%).
  • The elongation after fracture was 2.25 times that of the original sample.
  • Compared to the iron-doped AM50A (Fe) sample, the improvements were even more pronounced.
  • Structural Integrity Maintained: XRD analysis confirmed that the refining process did not damage the main characteristic peaks of the material, indicating structural integrity was preserved.

Limitations and Future Work

  • Limited to AM50A: The study focused specifically on AM50A magnesium alloy. While the principles might be applicable to other Mg alloys, further research would be needed to confirm this.
  • RJ-2 Agent Specificity: The study used a specific refining agent (RJ-2). Investigating other refining agents or developing new ones could offer alternative or improved solutions.
  • Cost-Effectiveness: While the process is effective, a detailed cost-benefit analysis of the refining agent and energy consumption would be beneficial for industrial scalability.
  • Future Work Suggestions: The authors implicitly suggest future work could involve exploring the application of this refined alloy in various industries and potentially investigating the long-term performance and corrosion resistance of the regenerated alloy. Further research into the exact mechanism of property enhancement by the refining agent could also be valuable.

Summary updated

Abstract

In recent years, the widespread application of Mg alloy casting and Mg alloy products has generated a large amount of Mg alloy waste. This experiment used a single factor experimental analysis method to study the optimal process for removing Fe from Mg alloy AM50A waste, and developed an efficient Fe removal and regeneration process for Mg alloy AM50A. It was found that the optimal refining temperature for removing Fe ions was 670 °C, the optimal refining (RJ-2) agent mass ratio was 1.5%, and the optimal refining time was 40 min. Regenerated J40-1.5-AM50A Mg alloy was prepared using the best refining process, and its composition and mechanical properties were tested and analyzed. The experimental results show that the composition of the regenerated J40-1.5-AM50A Mg alloy prepared by this method is consistent with AM50A, with an Fe removal rate of 96.2%. The mechanical properties were improved compared to the original AM50A sample, with a maximum tensile strength increase of 1.611 KN and a tensile strength increase of 26.333 MPa. The elongation after fracture is 2.25 times that of the original sample. Research has shown that the RJ-2 refining agent can provide mechanical properties of magnesium alloys during the refining process. By analyzing the composition, XRD, SEM, and EDS of AM50A (Fe) and J40-1.5-AM50A, it was found that the refining process accelerates the removal of Fe in the form of Fe deposition.
BibTeX
@inproceedings{zhao2024research,
  author = {Chen Zhao and Zhou Changfa and Wenbo Liu and Sanxing Chen and Gao Cong and Shaowei Jia and Xiaowen Yu and Zhou Wang and Bolin Luo and Qingshuang Zhang},
  title = {{Research on Fe Removal, Regeneration Process, and Mechanical Properties of Mg Alloy AM50A}},
  booktitle = {Crystals},
  year = {2024},
  doi = {10.3390/cryst14050407},
}
Figure