Regulation of the sintering trajectory of Ho,Pr:Y 2O 3 ceramics for 2.9 μm mid-infrared lasers by atmospheric sintering

Qing Li, Fei Liang, Jun Wang, Yanling Xue, Jie Ma, Peng Liu, Shiyu Sun, Hui Zhan, Jian Zhang, Changhua Zhang, Lili Hu, Haohai Yu, Huaijin Zhang, Dingyuan TangJournal of Advanced Ceramics 2024 · DOI

Introduction

Mid-infrared (MIR) lasers operating around 2.9 μm are essential for high-precision medical applications, such as "laser scalpels," and remote sensing. Holmium ($Ho^{3+}$) is a premier dopant for this range, but it faces a significant physical hurdle known as the self-termination effect. In $Ho^{3+}$, the lower laser energy level ($^5I_7$) has a much longer fluorescence lifetime than the upper level ($^5I_6$), creating a population bottleneck that prevents efficient lasing.

While codoping with Praseodymium ($Pr^{3+}$) can "drain" this lower level, fabricating the actual ceramic material is difficult. During the final stages of sintering, ceramic grains often grow too quickly, trapping microscopic pores inside the grains. These intragranular pores scatter light and ruin the transparency required for laser applications. Researchers have now developed a way to regulate this "sintering trajectory"—the relationship between grain size and density—to achieve near-theoretical transparency.

Sintering Methodology and Trajectory Control

The research team compared two primary sintering paths for $(Ho_{0.006}Pr_xY_{0.994-x})_2O_3$ powders: traditional vacuum presintering and a novel oxygen atmosphere presintering.

Sintering trajectory comparison: Grain size vs. relative density for vacuum and oxygen atmospheres.

As shown in the sintering trajectory data, the oxygen atmosphere acts as a "brake" for grain boundaries. In an oxygen-rich environment, the concentration of yttrium interstitials ($Y_i'''$)—the species controlling grain boundary movement—is reduced. This keeps grains small (average size <0.8 μm) while the material densifies. In contrast, vacuum sintering leads to abnormal grain growth and pore entrapment at the same temperatures. Furthermore, when $Pr$ is oxidized to $Pr^{4+}$ during oxygen sintering, its smaller ionic radius further inhibits grain boundary migration.

Optical Performance and Energy Transfer

Following presintering, all samples underwent Hot Isostatic Pressing (HIP) at 1450 °C and 200 MPa to reach full theoretical density. The oxygen-presintered ceramics achieved exceptional optical quality.

Transparent Ho,Pr:Y2O3 ceramic samples demonstrating high optical clarity over printed text.

The resulting ceramics achieved a transmittance exceeding 80% at 680 nm, which is very close to the theoretical limit for $Y_2O_3$. Spectroscopic analysis confirmed that the $Pr^{3+}$ deactivating ions effectively depopulated the lower $Ho^{3+}$ energy level. The addition of just 0.1 at% Pr slashed the lifetime of the problematic lower level from 11.52 ms to 3.80 ms, with an energy transfer efficiency reaching up to 93%.

Conclusion

By shifting from vacuum to oxygen atmosphere sintering, researchers successfully regulated the sintering trajectory of $Ho,Pr:Y_2O_3$ ceramics. This technique suppresses abnormal grain growth and eliminates trapped pores, resulting in highly transparent materials optimized for 2.9 μm laser emission. While the material properties are excellent, future work will focus on actual laser oscillation tests to measure real-world slope efficiency and output power.

Summary updated

Abstract

The sintering trajectory of the Ho,Pr:Y<sub>2</sub>O<sub>3</sub> ceramics could be effectively adjusted by sintering in a flowing oxygen atmosphere instead of vacuum. The final-stage grain growth was significantly suppressed by the use of oxygen atmosphere presintering, resulting in smaller average grain sizes than those of samples sintered under vacuum, while the same relative density was achieved. After hot isostatic pressing (HIP), the oxygen presintered Ho,Pr:Y<sub>2</sub>O<sub>3</sub> ceramics achieved excellent optical quality, with transmittance exceeding 80% at a wavelength of 680 nm. The codoping of Pr<sup>3+</sup> as deactivating ions effectively depopulated the lower energy level <sup>5</sup>I<sub>7</sub> during the Ho<sup>3+</sup>:<sup>5</sup>I<sub>6</sub> → <sup>5</sup>I<sub>7</sub> transition, thereby making the Ho,Pr:Y<sub>2</sub>O<sub>3</sub> ceramics more conducive to promoting population inversion in the 2.9 μm laser wavelength range.
BibTeX
@article{li2024regulation,
  author = {Qing Li and Fei Liang and Jun Wang and Yanling Xue and Jie Ma and Peng Liu and Shiyu Sun and Hui Zhan and Jian Zhang and Changhua Zhang and Lili Hu and Haohai Yu and Huaijin Zhang and Dingyuan Tang},
  title = {{Regulation of the sintering trajectory of Ho,Pr:Y <sub>2</sub>O <sub>3</sub> ceramics for 2.9 <strong>μ</strong>m mid-infrared lasers by atmospheric sintering}},
  journal = {Journal of Advanced Ceramics},
  year = {2024},
  doi = {10.26599/jac.2024.9221006},
}
Figure