Rapid Electrodeposition and Corrosion Behavior of Zn Coating from a Designed Deep Eutectic Solvent

Jiayi Chen, Mengjun Zhu, Mingtao Gan, Xiuli Wang, Changdong Gu, Jiangping TuMetals 2023 · DOI

TL;DR

Researchers have developed a novel deep eutectic solvent (DES) that significantly accelerates zinc electrodeposition onto mild steel, overcoming a major limitation of previous DES electrolytes. This new method yields dense, crack-free zinc coatings with superior corrosion resistance, particularly when deposited at 60°C and 4 mA/cm², paving the way for more efficient and industrial-scale zinc plating.

What Problem Does This Paper Address?

Traditional electrodeposition of zinc coatings, a crucial method for protecting mild steel from corrosion, often relies on aqueous electrolytes. While effective, these methods can have environmental drawbacks. Deep eutectic solvents (DESs) have emerged as promising alternatives due to their favorable properties like low volatility, biodegradability, and tunable polarity. However, a significant hurdle for the industrial application of many DESs, particularly those based on choline chloride (ChCl), is their slow electrodeposition rate. This slowness is attributed to factors like high liquid viscosity and limited metal ion solubility, which hinder mass transport. This paper tackles this challenge by designing a new DES formulation that enhances zinc ion concentration and reduces viscosity, thereby boosting the electrodeposition rate while maintaining or improving the quality and corrosion resistance of the zinc coating.

Methods

The researchers synthesized a novel DES by combining choline chloride (ChCl) with ethylene glycol (EG) and urea, and then incorporating a high concentration (up to 2 M) of zinc chloride (ZnCl₂). This DES was used as the electrolyte for electrodepositing zinc onto mild steel substrates.

Key experimental techniques employed include:

  • Cyclic Voltammetry (CV): Used to study the electrochemical behavior of the DES electrolyte at various temperatures (room temperature, 40°C, 60°C, and 80°C) to understand the underlying deposition mechanisms.
  • X-ray Diffraction (XRD): Employed to analyze the crystal structure and preferred orientation of the deposited zinc coatings under different electrodeposition conditions (temperature and current density).
  • Scanning Electron Microscopy (SEM): Utilized to characterize the surface morphology and cross-sectional structure of the zinc coatings, revealing details about their compactness, porosity, and adherence.
  • Energy Dispersive Spectrometry (EDS): Used in conjunction with SEM to confirm the elemental distribution and thickness of the zinc coating.
  • Tafel Polarization Curves and Electrochemical Impedance Spectroscopy (EIS): Standard electrochemical techniques used to evaluate the corrosion resistance of the zinc coatings in a 3.5 wt.% NaCl solution.

The study systematically varied electrodeposition temperature and current density to investigate their impact on coating properties.

Datasets

Not discussed in the paper. The study relies on experimental data generated from their own electrodeposition and characterization procedures.

Key Insights and Ideas

  • DES Design for Speed: The core innovation is the successful design of a DES that achieves a high zinc ion concentration (2 M) and maintains low viscosity, leading to a significantly faster electrodeposition rate compared to previous ChCl-based DES systems. This addresses a critical bottleneck for industrial adoption.
  • Temperature-Dependent Deposition Mechanism: The cyclic voltammetry results reveal a shift in the deposition mechanism with temperature. At lower temperatures, the DES behaves more like a urea-based system (fast nucleation, slow growth), while at higher temperatures, it exhibits characteristics of an EG-based system (slow nucleation, fast growth). This understanding is crucial for controlling coating morphology.
  • Crystal Orientation Dictates Morphology: The XRD analysis demonstrates a clear link between the dominant crystal plane (e.g., (002) vs. (101)) and the resulting zinc coating morphology. Lower temperatures favor (002) growth, leading to flatter coatings, while higher temperatures promote (101) growth, resulting in step-like structures.
  • Optimal Conditions for Corrosion Resistance: The study identifies specific conditions (60°C and 4 mA/cm²) that yield the most compact, crack-free zinc coatings with the best corrosion resistance. This is attributed to the dense morphology providing superior barrier protection.

Key Results

  • Rapid Electrodeposition: The developed DES achieved a deposition rate of nearly 15 µm in just 5 minutes at a current density of 12 mA/cm², a substantial improvement over existing DES methods.
  • Optimal Coating Morphology: The zinc coating deposited at 60°C and 4 mA/cm² exhibited the most compact and crack-free morphology.
  • Superior Corrosion Resistance: The coating produced under the optimal conditions (60°C, 4 mA/cm²) demonstrated the lowest corrosion current density (5.01 µA/cm²) and the highest polarization resistance (1053.11 Ω·cm²), indicating excellent corrosion protection. EIS results further corroborated this, showing the largest semicircle radius and highest impedance.
  • Influence of Parameters:
    • Temperature: Increasing temperature generally led to denser coatings up to 60°C, beyond which density decreased. Higher temperatures also shifted the corrosion potential to more negative values.
  • Current Density: Higher current densities led to smaller zinc particles and reduced surface flatness, with lower current densities generally resulting in better corrosion resistance.

Limitations and Future Work

  • Limited Temperature Range for Optimal Density: While 60°C yielded the densest coating, higher temperatures (80°C) led to decreased density, possibly due to electrolyte decomposition or water evaporation. Further optimization of temperature control might be beneficial.
  • Current Density vs. Corrosion Resistance: While the study found that lower current densities generally improve corrosion resistance, the paper notes that the effect of current density on corrosion resistance was less pronounced than that of temperature.
  • Future Work: The authors suggest that this work provides a foundation for the large-scale industrial application of DES in electrodeposition. Future research could focus on exploring a wider range of additives to further tailor coating properties, investigating the long-term performance of these coatings in various corrosive environments, and scaling up the electrodeposition process. The paper also mentions the possibility of further optimizing the DES composition for even higher zinc ion solubility and lower viscosity.

Summary updated

Abstract

This work aimed to develop a new type of deep eutectic solvent containing high concentrations of zinc ions as an electrolyte to improve the electrodeposition rate for zinc plating. Two typical deep eutectic solvent systems, choline chloride (ChCl)–urea and ChCl–ethylene glycol (EG), were combined to prepare a stable electrolyte at room temperature with a zinc ion concentration up to 2 M. Cyclic voltammetry experiments of the electrolyte at different temperatures were conducted. The effects of key electrodeposition parameters (bath temperature and current density) on the morphology, structure, and corrosion resistance of zinc coatings deposited on mild steel were investigated. It was found that the crystal orientation of the as-deposited zinc particle is related to the electrodeposition temperature and current density. The experimental results show that the zinc coating deposited at 60 °C and the current density of 4 mA·cm−2 exhibited the most compact and crack-free morphology, thus had the optimum corrosion resistance property.
BibTeX
@inproceedings{chen2023rapid,
  author = {Jiayi Chen and Mengjun Zhu and Mingtao Gan and Xiuli Wang and Changdong Gu and Jiangping Tu},
  title = {{Rapid Electrodeposition and Corrosion Behavior of Zn Coating from a Designed Deep Eutectic Solvent}},
  booktitle = {Metals},
  year = {2023},
  doi = {10.3390/met13010172},
}
Figure