Abstract
We investigate the scatter in the cycles to crack initiation for conventionally cast specimens of the superalloy RENE 80 in total strain controlled low cycle fatigue (LCF) tests at 850°C. The grains at the location of crack initiation are investigated using electron backscatter diffraction (EBSD) measurements with scanning electron microscopy (SEM). This results in determination of maximal Schmid factors for the slip system that lead to the initiation of the LCF surface crack. It is shown using stress - life and strain - life models, that taking into account the Schmid factor considerable reduces the scatter in LCF life prediction. This is used to propose a probabilistic model for LCF life based on random grain orientations. Using Mote Carlo simulation, we determine the probability distribution for the maximal Schmid factor in an uniaxial stress state under isotropic random orientations of the grain. This is used to calculate failure probabilities under the above mentioned model and to compare them with experimental data. Based on extreme value statistics, it is discussed whether a high maximal Schmid factor can be considered as causally related to an early initiation of an LCF crack and we present some rather surprising experimental evidence. In the last section conclusions are formulated and future directions of research are outlined.
Introduction
In the high-stakes environment of gas turbine engineering for aviation and power generation, predictability is essential. However, engineers face a significant hurdle: Low Cycle Fatigue (LCF) scatter. Even under strictly controlled laboratory conditions, the number of cycles until a crack initiates in coarse-grained superalloys like RENE 80 can vary by up to a factor of ten. This lack of predictability necessitates conservative maintenance schedules, which are economically inefficient. This study investigates the physical origins of this scatter, testing the hypothesis that the random orientation of individual crystal grains—quantified by the "Schmid factor"—is the primary driver of this statistical uncertainty.
Experimental Methodology
The researchers employed a multi-disciplinary approach using conventionally cast RENE 80. To account for statistical size effects, 40 specimens were tested across three distinct geometries (G1, G2, and G3), with surface areas ranging from approximately 44 $mm^2$ to 622 $mm^2$.
The material's microstructure is characterized by a coarse dendritic grain structure and a fine distribution of $\gamma/\gamma'$ precipitates, which significantly influence its mechanical response.
Total strain-controlled LCF tests were performed at 850°C. Following failure, Scanning Electron Microscopy (SEM) was used to locate the exact grain where the crack initiated. Electron Backscatter Diffraction (EBSD) then determined that specific grain's crystallographic orientation, allowing for the calculation of its Maximal Schmid Factor ($m$)—a measure of the resolved shear stress acting on the grain's slip planes.
Probabilistic Modeling
Standard life-prediction models (Ramberg-Osgood and Coffin-Manson-Basquin) were modified to incorporate $m$, effectively "correcting" the applied stress or strain based on local grain orientation. To understand the theoretical limits of this effect, the team ran $10^6$ Monte Carlo simulations to determine the probability distribution of Schmid factors in a material with perfectly random (isotropic) grain orientations.
Key Insights and Results
- Scatter Reduction: Adjusting fatigue life against "Schmid factor adjusted" stress or strain significantly tightened the data points. This confirms that local grain orientation is a dominant factor in determining crack initiation timing.
- The Magnitude Match: The variation in Schmid factors alone produces a predicted life scatter that matches the order of magnitude (roughly 10x) observed in experiments.
- The "Weakest Link" Paradox: Standard extreme value statistics suggest specimens should fail at the grain with the highest Schmid factor. However, experimental evidence showed that initiating grains did not have a strong bias toward high Schmid factors. At high strain levels, the distribution even shifted toward lower Schmid factors, suggesting that global plastification allows multiple slip systems to contribute to failure, making a single "bad" grain's orientation less decisive.
- Strain Dependency: The importance of the maximal Schmid factor grows as the strain amplitude decreases. At lower loads, specific grain orientation becomes a more critical trigger for failure.
Conclusion and Future Work
While Schmid factors explain much of the observed LCF scatter, they do not account for all of it. The study suggests that a "bad" grain orientation is a necessary but insufficient condition for early crack initiation; other local microstructural features must also align. Future research will investigate the relative orientation of activated slip systems to the specimen surface, the influence of neighboring grains (grain boundaries), and the specific configuration of the surrounding microstructure to refine these probabilistic models.
Summary updated