Abstract
This research investigates the development of a sustainable cementing agent (CA) for mine cemented paste backfill (CPB) using secondary smelting water-granulated nickel slag (SWNS) as the primary raw material. A composite activator consisting of flue gas desulphurization gypsum (FGDG), carbide slag (CS), $Na_2SO_4$, and cement clinker (CC) was optimized to trigger the latent hydraulic properties of the slag. The results demonstrate that a CA composition of 85% SWNS, 5% FGDG, 5% CS, 3% $Na_2SO_4$, and 2% CC achieves 28-day compressive and flexural strengths of 3.38 MPa and 1.99 MPa, respectively. These values meet the structural requirements for underground mining. Analysis via X-ray diffraction (XRD) and scanning electron microscopy (SEM) indicates that the hydration products, primarily ettringite (AFt) and calcium-magnesium-silicate-hydrate (C-M-S-H) gel, form through the activation of both vitreous and crystalline phases in the slag.
Introduction
In underground mining, Cemented Paste Backfill (CPB) is essential for filling voids to maintain structural stability. Traditionally, Ordinary Portland Cement (OPC) is the standard binder, but it is associated with high costs and significant $CO_2$ emissions. This study explores an eco-friendly alternative by utilizing secondary smelting water-granulated nickel slag (SWNS)—a byproduct of iron extraction—as a primary binder component. By "activating" this waste material with industrial byproducts, the research aims to reduce the environmental footprint and operational costs of mining backfill.
Materials and Methods
The experimental binder was composed of SWNS activated by a mixture of FGDG, CS, $Na_2SO_4$, and a small fraction of cement clinker. Iron ore tailings (IOT) served as the aggregate for the CPB material. The mineralogical characteristics of these raw materials were established using XRD analysis to identify reactive phases.
Mechanical properties were evaluated through compressive and flexural strength tests at 7 and 28 days. The hydration mechanism was further investigated using XRD and SEM to observe the formation of new mineral phases and the development of the material's microstructure over time.
Results and Discussion
Optimal Formulation and Strength
The study determined that the optimal ratio for the cementing agent is 85% SWNS, 5% FGDG, 5% CS, 3% $Na_2SO_4$, and 2% CC. This mixture yielded a 28-day compressive strength of 3.38 MPa, which is well within the 1–5 MPa range typically required for mine backfill applications.
Synergistic Activation and Hydration
The activation of SWNS is a multi-step process. Carbide slag (CS) provides the necessary alkalinity ($OH^-$ ions) to disrupt the stable glassy network of the nickel slag. Once the network is broken, the sulfate ions from the gypsum (FGDG) react with the released aluminum and calcium to form needle-like ettringite (AFt) crystals, providing early-stage reinforcement.
Furthermore, the study highlighted that both the glassy and crystalline phases of the SWNS contribute to strength. As shown in the XRD analysis of the raw materials, SWNS contains crystalline minerals such as monticellite and augite. The chemical activators facilitate the hydration of these phases, leading to the formation of C-M-S-H gel, which serves as the primary adhesive binding the tailings together. The addition of $Na_2SO_4$ further accelerates the process by increasing the system's pH more rapidly than traditional cement.
Conclusion
The use of secondary smelting nickel slag as a binder for mine backfill offers a viable path toward a circular economy in the mining industry. The developed composite activator successfully transforms industrial waste into a high-strength cementing agent that meets technical requirements while offering environmental and economic benefits. Future research should address the long-term durability of the CPB material and conduct comprehensive leaching tests to ensure the environmental safety of the immobilized slag.
Summary updated