Phytic-Acid-Modified Copper Foil as a Current Collector for Lithium-Ion Batteries

Mingtao Gan, Mengjun Zhu, Jiangping Tu, Xiuli Wang, Changdong GuMetals 2024 · DOI

TL;DR

Researchers have developed a novel, rapid electrodeposition method to coat copper foil current collectors with a thin layer of phytic acid (PA). This PA coating significantly enhances the copper foil's resistance to electrolyte corrosion and improves its adhesion to anode materials, leading to lithium-ion batteries with improved cycling stability, capacity retention, and rate performance.

What Problem Does This Paper Address?

Lithium-ion batteries (LIBs) are crucial for powering everything from our phones to electric vehicles. While much research focuses on the active materials within batteries, the current collectors—which conduct electricity and hold the active materials—are often overlooked. Standard copper foil, commonly used as an anode current collector, suffers from two main drawbacks: poor bonding with anode materials (like graphite) and susceptibility to corrosion by battery electrolytes. This corrosion can lead to detachment of the active material, increased interfacial resistance, and ultimately, a shorter battery lifespan and degraded performance. Existing solutions for modifying copper foil are often complex, time-consuming, or energy-intensive.

Methods

The core innovation in this paper is a fast electrodeposition process to apply a phytic acid (PA) film onto commercial electrolytic copper foil. This method is remarkably quick, taking only about 10 seconds. Here's a breakdown of the key techniques:

  • Electrodeposition: A two-electrode setup was used where the copper foil acted as the cathode and a copper plate as the anode. A plating solution containing sodium silicate, polyethylene glycol, and phytic acid was employed. When a current was applied, copper ions (Cu²⁺) from the anode chelated with phytic acid anions in the solution, forming an insoluble PA film that adhered to the copper foil cathode.
  • Characterization:
    • Scanning Electron Microscopy (SEM): Used to examine the surface morphology of the copper foil before and after PA treatment, and to observe the state of the electrodes after cycling.
  • Transmission Electron Microscopy (TEM): Employed to determine the precise thickness of the PA film.
  • Fourier-Transform Infrared Spectroscopy (FTIR): Used to confirm the presence of phytic acid on the copper foil.
  • X-ray Photoelectron Spectroscopy (XPS): Analyzed the surface composition of the copper foils after immersion in electrolyte to identify corrosion products and the effectiveness of the PA coating.
  • Electrochemical Impedance Spectroscopy (EIS): Measured interfacial resistance and charge transfer resistance.
  • Cyclic Voltammetry (CV): Assessed the electrochemical behavior of the electrodes.
  • Tafel Curves: Evaluated corrosion resistance.
  • Peel Strength Test: Quantified the bonding strength between the copper foil and the active anode material.
  • Battery Assembly and Testing:
    • Electrode Preparation: Artificial graphite, conductive carbon black, and PVDF binder were mixed with NMP solvent to form a slurry, which was then coated onto both pristine and PA-treated copper foils.
  • Half-Cell Assembly: The coated electrodes were assembled into half-type LIBs using lithium metal as the counter electrode, a standard electrolyte (1 M LiPF₆ in EC/DEC), and a Celgard separator.
  • Electrochemical Cycling: Batteries were subjected to various charge-discharge cycles at different current densities (0.1 A/g, 1 A/g, 2 A/g) to evaluate cycling stability, capacity retention, and rate performance.

Datasets

Not discussed in the paper. The study focuses on experimental characterization and electrochemical testing of modified copper foil.

Key Insights and Ideas

  • Phytic Acid as a "Smart" Coating: PA's strong chelating ability with metals is key. It forms a robust, thin (approx. 5 nm) protective layer that acts as a barrier against corrosive electrolyte components.
  • Rapid and Scalable Process: The 10-second electrodeposition is a significant advantage over traditional, time-consuming surface modification methods, making it potentially viable for industrial-scale production.
  • Dual Benefit: Corrosion Resistance and Adhesion: The PA film doesn't just protect the copper; it also actively improves the mechanical bonding between the copper foil and the graphite anode material. This is attributed to potential interactions between PA's functional groups and the anode material.
  • Reduced Interfacial Impedance: The improved bonding and reduced corrosion directly translate to lower interfacial and charge transfer resistances, crucial for efficient ion and electron transport within the battery.
  • Visible Corrosion Prevention: SEM images clearly show significantly less corrosion product formation on the PA-treated copper foil after prolonged electrolyte immersion compared to the pristine copper foil.

Key Results

  • Enhanced Bonding Strength: The bonding strength of graphite particles to PA-treated copper foil increased from 0.355 N cm⁻¹ to 0.441 N cm⁻¹ compared to pristine copper foil.
  • Improved Cycling Stability: At a low current density of 0.1 A/g, the PA-Cu electrode maintained a capacity retention of 85.6% after 400 cycles, significantly higher than the pristine Cu electrode's 57.5%.
  • Superior Rate Performance: At a high current density of 2 A/g, the PA-Cu electrode still delivered a capacity of ~115 mAh/g, whereas the pristine Cu electrode capacity dropped to ~80 mAh/g.
  • Corrosion Resistance: XPS analysis confirmed the presence of fewer corrosion products (like CuF₂, Cu(OH)₂) on the PA-Cu foil after 15 days of electrolyte immersion compared to the pristine Cu foil.
  • High Current Density Performance: At 1 A/g, the PA-Cu electrode showed a capacity retention of 85.9% after 500 cycles (compared to the 100th cycle), outperforming the pristine Cu electrode's 53.4% retention.

Limitations and Future Work

  • Electrolyte Wettability: While the PA film reduces electrolyte wettability on the copper foil surface (which contributes to corrosion resistance), the paper notes this effect. Further optimization might explore balancing this with optimal electrolyte interaction for anode material slurry application.
  • Long-Term Stability at Extreme Conditions: While impressive results were shown, further studies could investigate the performance under even more aggressive cycling conditions or over a larger number of cycles to fully understand the long-term durability.
  • Optimization of PA Film Properties: The paper mentions that PA film performance can be regulated by plating time, concentration, and pH. While optimal parameters were found for this study, further exploration of the PA film's properties (e.g., thickness, uniformity, chemical structure) under various conditions could lead to even greater improvements.
  • Application to Other Battery Chemistries: The study focused on graphite anodes for LIBs. Future work could explore the efficacy of PA-modified copper foil as a current collector for other anode materials (e.g., silicon, lithium metal) or even for cathode current collectors.

Summary updated

Abstract

Electrolytic copper foil is ideal for use in the anode current collectors of lithium-ion batteries (LIBs) because of its abundant reserves, good electrical conductivity, and soft texture. However, electrolytic copper foil is prone to corrosion in electrolytes and weak bonding to the anode substance. Surface modification of copper foil is considered an effective method of improving the overall electrochemical performance of LIBs. In this study, a 5 nm thickness phytic acid (PA)-based film is constructed on electrolytic copper foil using a fast electrodeposition process (about 10 s). PA-treated copper foil (PA-Cu) displays an improved corrosion resistance in electrolytes because of a strong complexation between the PA and copper. It is found that PA-treated copper foil also bonds better with graphite particles compared with pristine copper foil. LIBs with PA-Cu foils as their current collectors exhibit enhanced cycling stability, improved capacity retention, and superior rate performance at both low and high current densities. Our study offers a novel avenue for the development of high-performance electrode current collector materials for LIBs.
BibTeX
@inproceedings{gan2024phytic,
  author = {Mingtao Gan and Mengjun Zhu and Jiangping Tu and Xiuli Wang and Changdong Gu},
  title = {{Phytic-Acid-Modified Copper Foil as a Current Collector for Lithium-Ion Batteries}},
  booktitle = {Metals},
  year = {2024},
  doi = {10.3390/met14020247},
}
Figure