Magnetophoresis Assisted Capillary Assembly of Cobalt Nanorods: A New Source of Permanent Magnets for MEMS

Pierre Moritz, Fabrice Mathieu, David Bourrier, Daisuke Saya, Antoine Gonon, Liviu Nicu, Lise‐Marie Lacroix, Guillaume Viau, Thierry Leïchlé2020

TL;DR

This paper introduces a novel method for fabricating high-performance permanent magnets for MEMS devices by using magnetophoresis to guide the capillary assembly of cobalt nanorods. This technique allows for the creation of patterned, thick magnets at precise locations, paving the way for more integrated and powerful micro-electromechanical systems.

What Problem Does This Paper Address?

Micro-electromechanical systems (MEMS) that rely on electromagnetic actuation, such as sensors and energy harvesters, often require strong magnetic sources. Existing methods for creating permanent magnets (PMs) for MEMS have limitations: sputtering techniques produce high-performance magnets but are restricted to thin films and require high processing temperatures, making integration difficult. Electroplating offers thicker films at room temperature but yields significantly lower magnetic performance. Diluting magnetic microbeads in polymers can create thicker magnets, but their magnetic properties are moderate due to random particle orientation. There's a clear need for a method to fabricate thick (over 100 µm) PMs with high magnetic properties that are compatible with standard microfabrication processes and low temperatures.

Methods

The core innovation lies in the "magnetophoresis assisted capillary assembly" of cobalt nanorods (Co NRs).

  1. Cobalt Nanorod Synthesis: Co NRs are synthesized using a polyol process, resulting in crystalline nanorods approximately 250 nm long and 15 nm in diameter.
  2. Patterned Magnetic Structures: Nickel (Ni) blocks are electroplated onto silicon substrates to act as templates. These blocks are 150 µm thick and have specific footprints (e.g., 500x100 µm²).
  3. Magnetophoretic Assembly: A suspension of Co NRs in anisole is drop-cast onto the patterned Ni structures. While the suspension is applied, a strong external magnetic field (1 T) is used. This field magnetizes the Ni blocks, creating local magnetic field gradients. These gradients exert a magnetophoretic force on the Co NRs, attracting them to the Ni structures.
  4. Capillary Compaction: As the solvent evaporates, capillary forces further compact the attracted Co NRs, forming a dense magnetic material. The final geometry and thickness of the PM are dictated by the size and spacing of the Ni templates.

Datasets

Not discussed in the paper.

Key Insights and Ideas

  • Bottom-up Assembly for Precision: The combination of magnetophoresis and capillary forces offers a precise, bottom-up approach to pattern magnetic materials. This contrasts with top-down lithographic methods that can be limited in achievable thickness or material properties.
  • Synergy of Materials: The Ni blocks serve a dual purpose: they act as templates for assembly and contribute to the overall magnetic field of the final micro-magnet.
  • Low-Temperature Integration: The entire process is conducted at room temperature, making it highly compatible with existing MEMS fabrication flows, which often have temperature limitations.
  • Demonstrated Actuation: The paper successfully demonstrates that the fabricated micro-magnets are strong enough to actuate a silicon microcantilever at distances of several hundred micrometers, validating their practical utility.

Key Results

  • Thick Magnets: The method successfully fabricated permanent magnets with thicknesses up to 150 µm.
  • Magnetic Properties: The resulting Ni/Co NRs magnets exhibit a coercive field of 200 kA/m and a remanence induction of 0.3 T. The maximum energy product (BH)max is estimated at 14 kJ/m³.
  • Stray Field: The magnets produce a stray field of 30 mT at a distance of 100 µm and 14 mT at 200 µm.
  • MEMS Actuation: The fabricated magnets were able to actuate a silicon microcantilever, with the MEMS resonance frequency clearly observable even when the magnet was placed hundreds of micrometers away. The measured magnetic induction decay matched simulations.

Limitations and Future Work

  • Lower (BH)max than Ideal: The reported (BH)max of 14 kJ/m³ is lower than what has been achieved with similar Co NR assemblies in previous studies (e.g., [8,9]). The authors attribute this to the presence of the Ni blocks, which have a low coercive field, and the intertwining of longer Co NRs, which reduces the overall Co volume fraction.
  • Future Work: The authors suggest that this low-temperature, patterned fabrication method is well-suited for the direct monolithic integration of thick, high-performance permanent magnets into microelectronics and microsystems processes. Further optimization could focus on improving the (BH)max by addressing the factors mentioned above.

Summary updated

Abstract

International audience
BibTeX
@misc{moritz2020magnetophoresis,
  author = {Pierre Moritz and Fabrice Mathieu and David Bourrier and Daisuke Saya and Antoine Gonon and Liviu Nicu and Lise‐Marie Lacroix and Guillaume Viau and Thierry Leïchlé},
  title = {{Magnetophoresis Assisted Capillary Assembly of Cobalt Nanorods: A New Source of Permanent Magnets for MEMS}},
  year = {2020},
  doi = {10.1109/mems46641.2020.9056402},
}
Figure