Evolution of Calcareous Deposits and Passive Film on 304 Stainless Steel with Cathodic Polarization in Sea Water

Tianxiang Sun, Guosheng Huang, Ping Lv, Likun Xu, Li MaCoatings 2018 · DOI

TL;DR

This study investigates how cathodic polarization affects 304 stainless steel (SS) in seawater, focusing on calcareous deposit formation and passive film evolution. The findings reveal that a moderate potential of -0.50 V vs. SCE offers effective protection by promoting passive film growth without calcareous deposits, making it ideal for moving parts.

What Problem Does This Paper Address?

304 stainless steel is widely used in marine environments but is susceptible to localized corrosion like pitting and crevice corrosion due to chloride attack. While cathodic protection is a known effective method, achieving optimal protection requires careful consideration of the applied potential. Too little polarization offers insufficient protection, while excessive polarization can lead to issues like hydrogen embrittlement in some high-strength materials. Furthermore, cathodic protection can induce the formation of calcareous deposits, which are beneficial for stationary components by reducing current density and increasing protection duration, but undesirable for moving parts where smooth surfaces are crucial. This paper aims to elucidate the complex interplay between cathodic polarization potential, calcareous deposit formation, and passive film evolution on 304 SS in seawater to identify an optimized protection strategy.

Methods

The researchers employed a multi-faceted approach to characterize the surface evolution of 304 SS under cathodic polarization:

  • Potentiodynamic Polarization: This technique was used to determine the corrosion potential (Ecorr) and the potential range for effective cathodic protection, identifying the onset of oxygen reduction and hydrogen evolution.
  • Potentiostatic Polarization (Chronoamperometry): Samples were held at specific potentials (-0.50 V, -0.65 V, and -0.80 V vs. SCE) for extended periods, and the protective current density was measured over time to observe stabilization and changes.
  • Electrochemical Impedance Spectroscopy (EIS): EIS was employed at various time intervals to probe the changes in the passive film and calcareous deposits. Equivalent electrical circuits (EECs) were used to model the electrochemical processes occurring at the electrode-electrolyte interface.
  • Surface Analysis Techniques:
    • Scanning Electron Microscopy (SEM): Used to visualize the surface morphology and observe the formation, coverage, and structure of calcareous deposits.
  • Energy Dispersive X-ray (EDX) Microanalysis: Performed to determine the elemental composition of the surface and the calcareous deposits.
  • X-ray Diffraction (XRD): Utilized to identify the crystalline phases of the calcareous deposits.

Datasets

Not discussed in the paper. The study utilized natural seawater from the Yellow Sea as the test electrolyte and prepared 304 SS samples.

Key Insights and Ideas

  • Potential-Dependent Calcareous Deposit Formation: The formation of calcareous deposits is highly dependent on the applied cathodic potential. Deposits were observed at -0.80 V and -0.65 V but not at -0.50 V. This suggests a critical pH threshold for precipitation that is only reached at more negative potentials.
  • Dual Role of Calcareous Deposits: While beneficial for stationary parts by providing a protective barrier, the formation of calcareous deposits can be detrimental for moving components. The study highlights the need for a potential that balances protection with surface cleanliness.
  • Passive Film Dynamics: Cathodic polarization doesn't just lead to deposit formation; it also influences the passive film. At more negative potentials (-0.80 V and -0.65 V), the passive film initially degrades (indicated by decreased resistance) and then repairs itself due to the localized alkaline environment created by cathodic reactions.
  • Optimal Potential for Moving Parts: The potential of -0.50 V vs. SCE emerged as the optimal choice for protecting 304 SS, especially for moving parts. At this potential, the passive film grows and strengthens, providing good corrosion resistance without the formation of undesirable calcareous deposits.
  • Calcareous Deposit Composition Varies: The composition of calcareous deposits differed with potential. At -0.80 V, deposits contained CaCO3 and some Mg-containing substances, while at -0.65 V, only CaCO3 was detected. This difference is linked to the local pH achieved at each potential.

Key Results

  • Current Density: The protective current density was lower for maintaining polarization at -0.80 V than at -0.65 V, attributed to more compact calcareous deposits and a more resistant passive film at the former. The lowest current density was observed at -0.50 V, indicating efficient protection via passive film growth.
  • Calcareous Deposit Formation: Calcareous deposits were observed to form more readily and faster at -0.80 V compared to -0.65 V. At -0.50 V, no calcareous deposits were formed even after 168 hours of polarization.
  • Passive Film Resistance (Rox): For polarization at -0.80 V and -0.65 V, Rox initially decreased and then increased, indicating passive film reduction followed by repair. At -0.50 V, Rox continuously increased with polarization time, suggesting passive film growth and strengthening without reduction.
  • XRD Analysis: Aragonite (CaCO3) was identified as the primary phase of calcareous deposits formed at -0.80 V and -0.65 V. No Ca or Mg related substances were detected at -0.50 V.
  • SEM Morphology: Deposits at -0.80 V were initially coarse and corn-like, becoming more compact and thicker over time. At -0.65 V, deposits were more porous with gaps and holes. At -0.50 V, the surface remained clean.

Limitations and Future Work

  • Laboratory vs. Real-World: The authors acknowledge that the results were derived from laboratory testing. Engineering applications involve more complex factors like flow rate, temperature, seawater chemistry, and biofouling, which could influence the optimal potential.
  • Moving Parts Specificity: While -0.50 V is suggested for moving parts, further studies could specifically investigate the tribocorrosion behavior under this protection scheme.
  • Hydrogen Embrittlement: The study briefly mentions hydrogen embrittlement as a risk at very negative potentials. Further research could explore the threshold for this phenomenon on 304 SS under various conditions.
  • Long-Term Performance: While 168 hours of testing provides valuable insights, longer-term studies would be beneficial to confirm the sustained effectiveness of the proposed protection strategies.

Summary updated

Abstract

The change of protective current density, the formation and growth of calcareous deposits, and the evolution of passive film on 304 stainless steel (SS) were investigated at different potentials of cathodic polarization in sea water. Potentiostatic polarization, electrochemical impedance spectroscopy (EIS), and surface analysis techniques of scanning electron microscopy (SEM), energy dispersive X-ray (EDX) microanalysis and X-ray diffraction (XRD) were used to characterize the surface conditions. It was found that the protective current density was smaller for keeping polarization at −0.80 V (vs. saturated calomel electrode (SCE), same as below) than that at −0.65 V. The calcareous deposits could not be formed on 304 SS with polarization at −0.50 V while it was well protected. The formation rate, the morphology, and the constituent of the calcareous deposits depended on the applied potential. The resistance of passive film on 304 SS decreased at the first stage and then increased when polarized at −0.80 V and −0.65 V, which was related to the reduction and the repair of passive film. For the stainless steel polarized at −0.50 V, the film resistance increased with polarization time, indicating that the growth of oxide film was promoted.
BibTeX
@inproceedings{sun2018evolution,
  author = {Tianxiang Sun and Guosheng Huang and Ping Lv and Likun Xu and Li Ma},
  title = {{Evolution of Calcareous Deposits and Passive Film on 304 Stainless Steel with Cathodic Polarization in Sea Water}},
  booktitle = {Coatings},
  year = {2018},
  doi = {10.3390/coatings8050194},
}
Figure