Effects of Superfine Cement on Fluidity, Strength, and Pore Structure of Superfine Tailings Cemented Paste Backfill

Kunlei Zhu, Haijun Wang, Xulin Zhao, Luo Guanghua, Kewei Dai, Qinghua Hu, Yang Liu, Baowen Liu, Yonggang Miao, Jianbo Liu, Dingchao LvMinerals 2024 · DOI

TL;DR

This study explores how using superfine cement can improve the performance of cemented paste backfill (CPB) made with superfine mine tailings. The researchers found that superfine cement enhances fluidity, strength, and refines the pore structure of the backfill, offering a more sustainable solution for underground mining.

What Problem Does This Paper Address?

Underground mining operations generate vast amounts of mine tailings. To manage these tailings sustainably and improve mine safety, cemented paste backfill (CPB) is used to fill excavated voids. CPB typically consists of mine tailings, binders (like cement), and water. However, advancements in mining have led to an increase in "superfine" tailings, which have very small particle sizes and a high surface area. While this can be beneficial in some ways, it also presents challenges: these superfine tailings require more water, which can negatively impact the fluidity (how easily it flows) and the ultimate strength of the CPB. This makes it difficult to transport and use effectively in underground applications. This paper aims to address these limitations by investigating the use of superfine cement as a binder to improve the properties of CPB made with superfine tailings, a material referred to as STCPB.

Methods

The researchers prepared STCPB samples using superfine tailings, superfine cement, and deionized water. They systematically varied the cement-to-tailings ratio (CTR) and solid content (SC) to study their effects.

Key experimental methods included:

  • Fluidity Test: Measured by the spread diameter (SD) of the fresh STCPB slurry using a standard conical mold.
  • Unconfined Compressive Strength (UCS) Test: Assessed the mechanical strength of hardened STCPB specimens using a universal testing machine.
  • Packing Density and Water Film Thickness (WFT) Test: Determined the packing density of the solid particles and calculated the water film thickness (WFT) around the particles, a crucial factor influencing rheology.
  • Mercury Intrusion Porosimetry (MIP) Test: Analyzed the pore structure of the hardened STCPB, including porosity and pore size distribution.

The study also employed statistical analysis, fitting various models (linear, exponential, logarithmic) to the experimental data to quantify the relationships between different parameters (CTR, SC, WFT) and the observed properties (fluidity, strength, pore structure).

Datasets

Not discussed in the paper. The study relies on experimental data generated from prepared STCPB samples.

Key Insights and Ideas

  • Superfine Cement is a Game Changer: The core idea is that using superfine cement (similar in fineness to the superfine tailings) can overcome the limitations imposed by the fine tailings themselves. This is a clever approach to match the binder's particle size to the aggregate's particle size for better performance.
  • Water Film Thickness (WFT) is Key to Fluidity: The study highlights WFT as a critical factor for fluidity. A thicker water film means less friction between particles, leading to better flow. This is intuitive but quantifying it for STCPB is important.
  • WFT's Dual Role in Strength: WFT has a complex, non-linear effect on strength. Low WFT promotes strong particle bonding, moderate WFT balances hydration and flow, while high WFT hinders hydration and reduces strength. This suggests an optimal WFT window for maximum strength.
  • Pore Structure Refinement: Superfine cement significantly reduces porosity and, importantly, the proportion of larger pores (macropores) in the STCPB. This is a direct consequence of better particle packing and more efficient hydration.

Key Results

  • Fluidity:
    • Increasing the cement-to-tailings ratio (CTR) decreases fluidity (spread diameter).
  • Increasing the solid content (SC) also decreases fluidity.
  • Water film thickness (WFT) has a strong exponential positive correlation with fluidity (SD). An increase in WFT from 0.001 to 0.041 µm increased SD from 20.63 to 37.68 cm.
  • Strength (UCS):
    • Both CTR and SC show exponential relationships with UCS, with higher values leading to increased strength. This is attributed to more hydration products and reduced porosity.
  • WFT has a complex, non-linear effect on UCS. Low WFT (0-0.0071 µm) enhances strength by promoting hydration and bonding. Moderate WFT (0.0071-0.0193 µm) balances hydration and flowability. High WFT (>0.0193 µm) reduces hydration efficiency and strength.
  • Pore Structure:
    • STCPB prepared with superfine cement showed lower porosity (43.4% for STCPB-1 vs. 47.6% for STCPB-2, which used OPC) and a significantly lower proportion of macropores compared to a reference sample using ordinary Portland cement (OPC).

Limitations and Future Work

The authors acknowledge several limitations:

  • Long-Term Performance: The study did not include long-term strength and durability testing under real-world conditions. This is crucial for evaluating the material's behavior over extended periods.
  • Economic and Environmental Impact: While superfine cement offers potential benefits, its economic feasibility and environmental impact for large-scale applications require further investigation.

Future work suggested includes:

  • Focusing on long-term performance and durability studies.
  • Conducting detailed economic and environmental impact assessments for large-scale implementation.
  • Further exploring the practical implications of using superfine cement in mine backfilling operations.

Summary updated

Abstract

Advancements in mine tailings treatment technology have increased the use of superfine tailings, but their extremely fine particle size and high specific surface area limit the performance of superfine tailings cemented paste backfill (STCPB). This study investigates the effects of using superfine cement as a binder to enhance the fluidity, strength, and pore structure of STCPB. The influence of water film thickness (WFT) on STCPB performance is also examined. The results show that the cement-to-tailings ratio (CTR) and solid content (SC) significantly affect the spread diameter (SD) and unconfined compressive strength (UCS), following distinct linear/logarithmic and exponential trends, respectively. WFT has an exponential impact on SD and a non-linear effect on UCS, enhancing strength at low levels (0 μm < WFT < 0.0071 μm) and balancing hydration and flowability at moderate levels (0.0071 μm < WFT < 0.0193 μm) but reducing strength at high levels (WFT > 0.0193 μm). Additionally, superfine cement significantly improves the pore structure of STCPB by reducing porosity and macropore content. These findings provide valuable insights into optimizing STCPB for enhanced performance and sustainability in mine backfilling applications.
BibTeX
@inproceedings{zhu2024effects,
  author = {Kunlei Zhu and Haijun Wang and Xulin Zhao and Luo Guanghua and Kewei Dai and Qinghua Hu and Yang Liu and Baowen Liu and Yonggang Miao and Jianbo Liu and Dingchao Lv},
  title = {{Effects of Superfine Cement on Fluidity, Strength, and Pore Structure of Superfine Tailings Cemented Paste Backfill}},
  booktitle = {Minerals},
  year = {2024},
  doi = {10.3390/min15010024},
}
Figure