Effect of Ti3SiC2 Amount on Microstructure and Properties of TiAl Matrix Composites

Qin Zou, Zhichao Lou, Yong Guan, Yanguo Li, Jiangbo Xu, Yuanyuan Li, Lingyu Bu, Peng Wang, Yongan LuoResearch 2021 · DOI

Introduction

Titanium Aluminum (TiAl) alloys have emerged as critical materials for the aerospace and automotive sectors, primarily due to their low density and high-temperature strength. These properties make them ideal for components such as turbine blades and turbochargers. However, TiAl alloys suffer from significant tribological limitations, including high friction coefficients and poor wear resistance. Traditional liquid lubricants are ineffective at the elevated operating temperatures typical for these alloys, as they tend to oxidize or decompose.

To address these challenges, researchers are investigating self-lubricating composites. One promising additive is $Ti_3SiC_2$, a member of the "MAX phase" ceramics. These materials combine the beneficial properties of metals—such as electrical and thermal conductivity and thermal shock resistance—with the stiffness and heat resistance of ceramics. This study evaluates the impact of varying $Ti_3SiC_2$ concentrations on the microstructure, mechanical strength, and wear behavior of TiAl matrix composites at both room temperature and 550°C.

Methodology

The composites were synthesized using Spark Plasma Sintering (SPS), a technique that utilizes pulsed direct current to achieve rapid densification. Sintering was conducted at 1100°C for 10 minutes under a pressure of 30 MPa. Four distinct compositions were prepared:

  • TA0: Pure TiAl (control).
  • TA1: TiAl + 10 wt.% $Ti_3SiC_2$.
  • TA2: TiAl + 20 wt.% $Ti_3SiC_2$.
  • TA3: TiAl + 30 wt.% $Ti_3SiC_2$.

The resulting materials were characterized using X-ray diffraction (XRD) and Field Emission Scanning Electron Microscopy (FESEM) paired with Energy Dispersive Spectroscopy (EDS) to determine phase composition and microstructure. Mechanical testing included Vickers hardness measurements and compression testing via Gleeble systems. Tribological performance was assessed using pin-on-disc tests to measure friction coefficients and wear rates at room temperature and 550°C.

Microstructural Evolution

A key finding of the study is that $Ti_3SiC_2$ does not remain inert within the TiAl matrix. During the high-temperature sintering process, the $Ti_3SiC_2$ partially decomposes, leading to the formation of $Ti_5Si_3$ and $TiC$ phases. These secondary phases are crucial as they act as reinforcing "pins" at the grain boundaries, significantly enhancing the material's resistance to deformation. While $Ti_3SiC_2$ was generally distributed homogeneously, the researchers noted that higher concentrations (approaching 30 wt.%) began to show signs of agglomeration, which can introduce localized porosity.

Mechanical and Tribological Performance

The addition of $Ti_3SiC_2$ significantly improved the mechanical properties of the TiAl matrix. The TA3 (30 wt.%) composite demonstrated the best overall performance:

  • Hardness: Reached 5.1 GPa.
  • Compression Strength: Peaked at 1080 MPa at room temperature and 640 MPa at 550°C.
  • Wear Resistance: At 550°C, the TA3 sample exhibited a friction coefficient of 0.423 and a wear rate of $0.21 \times 10^{-4} \text{ mm}^3\text{N}^{-1}\text{m}^{-1}$.

Interestingly, the composites performed better at 550°C than at room temperature. This "inverse" temperature effect is attributed to the nature of the lubricating films formed during friction. At room temperature, a thin film of $Ti_3SiC_2$ provides lubrication, primarily through abrasive wear mechanisms. However, at 550°C, a complex Fe-Ti-Al-Si-oxide film forms on the surface. This oxide layer is more stable and effective at reducing friction and wear, shifting the primary wear mechanism toward adhesive wear.

Conclusion and Future Directions

The study concludes that 30 wt.% $Ti_3SiC_2$ is the optimal concentration for enhancing the tribological and mechanical properties of TiAl composites via SPS. The formation of a high-temperature oxide lubricating film provides a robust solution for wear protection in extreme environments.

Future research should focus on:

  1. High-Temperature Limits: Testing beyond 550°C to determine the breakdown point of the oxide film.
  2. Particle Engineering: Utilizing finer $Ti_3SiC_2$ powders to mitigate agglomeration and potentially allow for higher loading.
  3. Fatigue Testing: Evaluating the material's durability under cyclic loading conditions, which is essential for aerospace certification.

Summary updated

Abstract

Abstract The TiAl matrix composites were manufactured using spark plasma sintering under the conditions of 1100 °C/10 min/30 MPa. The effect of Ti 3 SiC 2 amount on microstructure and properties of TiAl matrix composites was investigated. Ti 3 SiC 2 was homogeneously distributed in the TiAl matrix, and it partly decomposed to form Ti 5 Si 3 and TiC. The TiAl matrix with 30 wt.% of Ti 3 SiC 2 exhibited the lowest friction coefficient and wear rate of 0.507 and 1.35´10 -4 mm 3 N -1 m -1 at room temperature and 0.423 and 0.21´10 -4 mm 3 N -1 m -1 at 550 °C, while the compression strength reached the maximum value of 1080 GPa at room temperature and 640 GPa at 550 °C, respectively. The hardness reached the value of 5.1 GPa. The TiAl matrix composites had a lower friction coefficient and wear rate at 550 °C than at room temperature. A Ti 3 SiC 2 lubricating film was formed on the friction surface of the TiAl matrix composites after friction test at room temperature, while a Fe-Ti-Al-Si-oxide lubricating film was formed after friction test at 550 °C. The wear mechanisms of the TiAl matrix composites with the Ti 3 SiC 2 addition were mainly abrasive wear and adhesive wear at room temperature and 550 °C, respectively.
BibTeX
@inproceedings{zou2021effect,
  author = {Qin Zou and Zhichao Lou and Yong Guan and Yanguo Li and Jiangbo Xu and Yuanyuan Li and Lingyu Bu and Peng Wang and Yongan Luo},
  title = {{Effect of Ti3SiC2 Amount on Microstructure and Properties of TiAl Matrix Composites}},
  booktitle = {Research},
  year = {2021},
  doi = {10.21203/rs.3.rs-1050375/v1},
}

Loading related content...

Figure