Effect of the mould pressure on tribological property of carbon/phenolic resin composites

Yue Cao, Midan Li, Han Liu, Mengyi Cao, Jiawei Wang, Yue Wang, Yijia Deng2015 · DOI

Abstract

The carbon/phenolic resin composites, consisting of phenolic resin, natural graphite, and carbon fiber, were fabricated by hot compression moulding. This study investigates the effects of mould pressure on the tribological properties of these composites. Results indicate that as mould pressure increases from 20 MPa to 40 MPa, hardness increases while the friction coefficient and wear rate decrease. Beyond 40 MPa, these properties change only slightly. At the optimal pressure of 40 MPa, the composites exhibited a hardness of 64 HS, a friction coefficient of 0.18, and a wear rate of 1.94 × 10⁻⁶ mm³ N⁻¹ m⁻¹. The superior wear resistance at 40 MPa is attributed to high material hardness and the formation of a complete transfer film.

Introduction

Carbon/polymer composites are essential in high-performance engineering applications, such as aircraft bearings and automotive braking systems. These materials typically combine a resin matrix with lubricating graphite and reinforcing carbon fibers. However, a significant challenge in their fabrication is the presence of microscopic voids or "gaps" that occur when high concentrations of fillers make the mixture extremely viscous. These internal defects weaken the material, causing reinforcing fibers to loosen or snap during operation, which leads to high friction and rapid failure. This research explores how varying the mould pressure during hot compression can mitigate these defects and optimize tribological performance.

Experimental Methods

The composites were prepared using a liquid resol-type phenolic resin reinforced with natural graphite flakes and polyacrylonitrile (PAN)-based carbon fibers. The fabrication process involved mechanical mixing at 3000 rpm for 10 minutes, followed by hot compression moulding at 180°C. Four different mould pressures were tested: 20, 30, 40, and 50 MPa, with a holding time of 1.5 hours.

The resulting materials were characterized using several techniques:

  • Tribological Testing: A block-on-ring tribometer measured friction and wear under dry sliding conditions (150 N load, 400 rpm).
  • Hardness Testing: Shore hardness (HS) was determined using a diamond ball indenter.
  • Morphological Analysis: Scanning Electron Microscopy (SEM) was employed to examine the worn surfaces and understand the underlying wear mechanisms.

Results and Discussion

Effect of Pressure on Hardness

Increasing the mould pressure from 20 to 40 MPa significantly improved the compaction of the composite. Higher pressure effectively eliminates internal voids, leading to a more continuous and robust matrix. As shown in the data, the Shore hardness increased from 45 HS at 20 MPa to a peak of 64 HS at 40 MPa. Interestingly, increasing the pressure further to 50 MPa resulted in a slight decrease in hardness, suggesting a threshold where the material is fully compacted or where excessive pressure might begin to degrade the structural integrity of the components.

Hardness (HS) of carbon/phenolic resin composites as a function of mould pressure.

Tribological Performance and the Transfer Film

The tribological properties showed a strong correlation with the fabrication pressure. The friction coefficient dropped from 0.25 at 20 MPa to 0.18 at 40 MPa. More dramatically, the wear rate was reduced by approximately 53%, falling from 4.12 to 1.94 × 10⁻⁶ mm³ N⁻¹ m⁻¹.

Wear rate of carbon/phenolic resin composites at various mould pressures.

The primary mechanism for this improvement is the formation of a stable "transfer film." At lower pressures (e.g., 20 MPa), weak bonding between the fibers and the resin allows fibers to break away easily. These fragments act as abrasive debris, preventing the formation of a smooth lubricating layer. At 40 MPa, the increased density and bonding strength facilitate the creation of a complete transfer film on the sliding surface, which protects the composite and reduces direct contact with the counter-face.

Conclusion

This study identifies 40 MPa as the optimal mould pressure for manufacturing carbon/phenolic resin composites. At this pressure, the material achieves a balance of high hardness and excellent wear resistance. While increasing pressure up to 40 MPa yields significant benefits, further increases to 50 MPa offer diminishing returns and a slight reduction in hardness. Future work should investigate the specific causes of performance degradation at extreme pressures and evaluate the material's durability under varying environmental conditions and long-term fatigue cycles.

Summary updated

Abstract

The carbon/phenolic resin composites consist of phenolic resin, natural graphite and carbon fiber, were fabricated by hot compression moulding. The effects of the mould pressure on tribological property of carbon/phenolic resin composites were investigated. The results indicated that the hardness increased, the friction coefficient and wear rate decreased with increasing mould pressure from 20 Mpa to 40 Mpa, further increasing mould pressure the hardness and the wear resistance of composites changed slightly. The hardness, friction coefficient and wear rate of composites at 40 Mpa were 64, 0.18 and 1.94 10 -6 mm 3 N -1 m -1 , respectively. The high hardness and complete transfer film were conttributed to good wear resistance of composites fabricated at 40MPa.
BibTeX
@misc{cao2015effect,
  author = {Yue Cao and Midan Li and Han Liu and Mengyi Cao and Jiawei Wang and Yue Wang and Yijia Deng},
  title = {{Effect of the mould pressure on tribological property of carbon/phenolic resin composites}},
  year = {2015},
  doi = {10.2991/iccet-15.2015.337},
}