Effect of Polyvinylpyrrolidone Content on Pure Titanium Injection Molding

Weichen Zhang, Lü Li, Chuanyong Li, Yanhua Sun, Muhammad Dilawer Hayat, Yugeng Li, Gang Chen, Zhentao Yuan, Xiao WangCrystals 2023 · DOI

TL;DR

This paper tackles the challenge of pore formation in pure titanium injection molding using a water-soluble binder system. By incorporating Polyvinylpyrrolidone (PVP) as a crystallization inhibitor, the researchers successfully reduced defects and significantly improved the mechanical properties of the final titanium parts, with 20 wt.% PVP proving to be the optimal concentration.

What Problem Does This Paper Address?

Metal Injection Molding (MIM) is a powerful technique for creating complex, near-net-shape metal parts. However, when using water-soluble binder systems like Polyethylene Glycol (PEG) and Polymethylmethacrylate (PMMA) for pure titanium, a critical issue arises: the difference between PEG's crystallization temperature and PMMA's glass transition temperature leads to pore formation during solidification. These pores severely degrade the mechanical properties of the final sintered parts, limiting the application of this otherwise clean and efficient MIM process for titanium. This study aims to overcome this challenge by introducing a crystallization inhibitor to the binder system.

Methods

The researchers employed a multi-step approach to investigate the effect of PVP on titanium MIM:

  • Feedstock Preparation: Spherical pure titanium powder (less than 45 µm) was mixed with a binder system composed of PEG, PMMA, and Sodium Alginate (SA). Different weight percentages of PVP (0%, 10%, 20%, and 30%) were added to this binder. The mixture was compounded at 160 °C for 90 minutes.
  • Injection Molding: A desktop pneumatic injection molding machine was used with specific parameters (barrel temperature 160 °C, nozzle 165 °C, mold 50 °C, injection pressure 0.8 MPa, holding time 5 s).
  • Debinding:
    • Water Debinding: Performed at 50 °C to remove PEG and PVP, creating open channels for subsequent thermal debinding.
  • Thermal Debinding: Conducted in a vacuum sintering furnace.
  • Sintering: Samples were sintered at 1300 °C for 2 hours in a vacuum sintering furnace. A specific holding time at 380 °C was included to manage the escape of decomposition gases.
  • Characterization:
    • SEM (Scanning Electron Microscopy): Used to observe the morphology of the feedstock, injection-molded samples, and water-debonded samples, as well as the fracture surfaces of sintered parts.
  • Micro CT (Micro-Computed Tomography): Employed to visualize the internal pore structure before and after water debinding.
  • DSC (Differential Scanning Calorimetry): Analyzed the crystallization behavior of PEG and the effect of PVP.
  • TGA (Thermogravimetric Analysis): Studied the thermal decomposition of the binder system.
  • Rheology: Measured the shear viscosity of the feedstocks to assess their suitability for injection molding.
  • Mechanical Testing: Ultimate tensile strength, elongation, and relative density of the sintered samples were determined using an MTS universal tester.
  • Impurity Analysis: ICP-OES was used to quantify impurity content.

Datasets

Not discussed in the paper. The study utilizes experimental materials (titanium powder and binder components) and generates its own data through experiments and characterization.

Key Insights and Ideas

  • PVP as a Pore Inhibitor: The core idea is that PVP acts as a crystallization inhibitor for PEG. By compressing the crystallization space of PEG molecules, PVP prevents the inconsistent volume shrinkage that occurs during cooling, thereby reducing pore formation.
  • Optimal PVP Concentration: The study reveals a sweet spot for PVP concentration. While adding PVP generally reduces pores, too much (30 wt.%) can lead to defects like cracks due to internal stresses. Conversely, insufficient PVP (10 wt.%) still leaves some pores. 20 wt.% PVP emerged as the optimal level for achieving defect-free samples.
  • Binder System Performance: The PEG/PMMA/SA binder system, enhanced with 20 wt.% PVP, demonstrated good rheological properties and feedstock uniformity, crucial for successful injection molding.
  • Water Debinding's Role: Water debinding is essential for creating interconnected open channels, facilitating the removal of binder components during thermal debinding and minimizing risks like cracking and blistering.
  • Trade-off with Impurities: While PVP improves mechanical properties, it also slightly increases impurity content. This highlights the need to balance defect reduction with material purity.

Key Results

  • Pore Reduction: SEM images clearly show a significant reduction in pores with increasing PVP content, with near-pore-free surfaces observed at 20 wt.% PVP.
  • Improved Mechanical Properties: The ultimate tensile strength increased from 386.4 MPa (0% PVP) to a peak of 547.9 MPa at 20 wt.% PVP. Elongation also improved from 8.83% to 12.53%.
  • Density: The relative density of sintered samples reached 98.6% at 20 wt.% PVP, meeting the requirements for ASTM F2989-13 Grade 3.
  • Rheological Suitability: All feedstocks exhibited shear viscosities below 1000 Pa·s in the tested range, indicating suitability for injection molding.
  • Debinding Behavior: Water debinding rate was highest without PVP, but PVP addition did not hinder the overall removal of PEG and PVP within 24 hours. However, 30 wt.% PVP led to sample destruction due to cracks.

Limitations and Future Work

  • Impurity Increase: The study notes that increasing PVP content leads to a slight increase in impurity levels (C, O, N). While the 20 wt.% PVP sample still met standards, further optimization might be needed to minimize this.
  • 30 wt.% PVP Failure: The 30 wt.% PVP feedstock resulted in cracked and destroyed samples, indicating an upper limit for PVP addition. The exact mechanism of this failure and how to mitigate it could be explored.
  • Binder Composition Optimization: While PEG/PMMA/SA with PVP was investigated, further research could explore variations in the base binder composition or the use of different crystallization inhibitors.
  • Specific Application Focus: The study focuses on pure titanium. Extending this research to titanium alloys or other challenging-to-process metals could be a valuable future direction.
  • Long-term Stability: While mechanical properties are reported, long-term stability and performance in specific applications are not discussed.

Summary updated

Abstract

In water-soluble binder systems, polyethylene glycol (PEG) and polymethylmethacrylate (PMMA) are often used as primary and secondary components. The PEG/PMMA binder system is clean and environmentally friendly, but the discrepancy between the crystallization temperature of PEG and the glass transition temperature of PMMA leads to the generation of pores in the feedstock. The solidification pores have an adverse impact on the final mechanical properties of the samples. Polyvinylpyrrolidone (PVP), as a crystallization inhibitor, can inhibit the formation of porosity. In this study, spherical titanium powder with a diameter of less than 45 μm was used as metal powder; the binder system consisted of PEG, PMMA and SA. Different increments of PVP (0, 10%, 20%, 30 wt.%) were added to the PEG/PMMA binder system. The uniformity of the feedstock and the open channels generated after debinding were observed using SEM. The pores’ condition before and after debinding was studied using Micro CT, and the mechanical properties of the samples were also detected. By comparing the macroscopic and microscopic morphologies of the injected samples and mechanical properties of the sintered samples, it was found that a PVP content of 20 wt.% resulted in the best properties.
BibTeX
@inproceedings{zhang2023effect,
  author = {Weichen Zhang and Lü Li and Chuanyong Li and Yanhua Sun and Muhammad Dilawer Hayat and Yugeng Li and Gang Chen and Zhentao Yuan and Xiao Wang},
  title = {{Effect of Polyvinylpyrrolidone Content on Pure Titanium Injection Molding}},
  booktitle = {Crystals},
  year = {2023},
  doi = {10.3390/cryst13111563},
}
Figure