Abstract: Composite insulators have been widely used for transmission lines, which have been noted for the aging problem with the increase of the installed number and service time. Characteristics analysis of aging composite insulators were analyzed using attenuated total reflection infrared spectroscopy (ATR-FTIR) and thermogravimetric analysis (TGA) respectively. Results showed that the aging rate of composite insulators were increased by higher voltage and longer operation period, and molecular fracture was the main performance of aging. It was suggested that sheds materials for composite insulators of various aging degree shows good thermostability without significant difference.
Introduction
Since the 1980s, composite insulators—primarily made of high-temperature vulcanized (HTV) silicone rubber—have become the backbone of high-voltage transmission lines. Favored over traditional glass or ceramic for their lightweight nature and superior hydrophobicity, these polymers prevent electrical arcing in diverse environments. However, as many of these components approach the end of their 30-year design life, understanding the chemical mechanisms of their degradation is critical for grid reliability.
This study investigates the "aging" of these materials, which involves the chemical breakdown of polymer chains. By quantifying how factors like operating voltage, service duration, and environmental conditions (such as coastal salt spray versus urban smog) degrade the molecular structure of the insulator's "sheds," researchers can better predict maintenance needs.
Methodology
The research utilized two primary analytical techniques to probe the insulator samples:
- ATR-FTIR (Attenuated Total Reflection Fourier Transform Infrared Spectroscopy): This technique serves as a chemical "fingerprint" scanner. By measuring the absorption peaks of specific chemical bonds, such as Si-CH₃ (methyl groups) and Si-O-Si (the polymer backbone), the team could detect "molecular fracture"—the literal breaking of the polymer chains.
- TGA (Thermogravimetric Analysis): To assess bulk durability, samples were heated to 800°C. Measuring the temperature and magnitude of weight loss during decomposition allowed researchers to determine the material's thermal stability over years of field use.
Molecular Degradation Analysis
The core of the insulator is HTV silicone rubber, specifically polydimethylsiloxane (PDMS). Its chemical structure consists of a repeating siloxane (Si-O-Si) backbone with methyl (CH₃) side groups that provide the material's characteristic water-repellency.
Voltage Stress and Terminal Aging
A key finding of the spectroscopic analysis is that aging is not uniform across the insulator. The high-voltage terminal, which experiences the highest electric field intensity, shows the most significant molecular degradation. In 220kV samples, the absorption peaks for Si-CH₃ and Si-O-Si were significantly smaller at the high-voltage terminal compared to the low-voltage terminal, confirming that electrical stress directly correlates to bond breakage.
Environmental Impacts and Thermal Stability
Environment plays a decisive role in the rate of degradation. Insulators located in peri-urban and industrial areas—characterized by high anthropogenic contamination—showed deeper aging than those in rural plains or coastal areas. This suggests that industrial particulates and smog act as catalysts for the breakdown of silicone rubber.
Interestingly, the study revealed a decoupling between surface chemistry and bulk thermal properties. While the surface molecules clearly fracture over time, the material's ability to withstand high heat remains remarkably stable. The 5% weight loss temperature for a new insulator was recorded at 333.6°C; after 8 years of service, this only slightly decreased to 324.2°C. This indicates that while the surface degrades, the bulk material does not undergo a catastrophic qualitative change in its first decade of use.
Conclusion
The analysis concludes that molecular fracture is the primary mechanism of aging in composite insulators, driven largely by high voltage stress and environmental pollution. Despite these chemical changes, the insulators maintain high thermostability. Future research should aim to correlate these chemical fractures with mechanical integrity and hydrophobicity loss to provide a more comprehensive prediction of the service life for insulators exceeding 20 years of operation.
Summary updated