TL;DR

This paper presents a robust, integrated workflow for calibrating spherical nanoindentation instruments and analyzing the resulting data. By developing a method to accurately determine the effective tip radius and machine stiffness as a function of load, the authors enable more reliable extraction of stress-strain curves and material properties, particularly for materials with complex deformation behaviors.

What Problem Does This Paper Address?

Spherical nanoindentation is a powerful technique for probing material properties at the micro- and nanoscale. However, accurately interpreting the load-displacement data is challenging due to several factors: the complex stress field induced by a spherical tip, the need for precise calibration of the indenter tip's shape (effective radius), and the influence of the instrument's own stiffness (machine stiffness). Existing methods for calibration often rely on assumptions or single-point measurements that can lead to systematic errors, especially when dealing with materials exhibiting plasticity or when comparing data across different instruments. This paper addresses the need for a self-consistent, reliable, and integrated approach to calibrate spherical nanoindentation systems and extract accurate material properties, particularly stress-strain curves and yield points.

Methods

The authors propose a comprehensive calibration routine that integrates and adapts existing methodologies. Key aspects include:

  • Load-Dependent Effective Tip Radius: Instead of assuming a constant effective tip radius, they parameterize it as a function of load. This is achieved by analyzing the differences in displacement data obtained from multiple reference materials (fused silica, sapphire, glassy carbon) at the same applied load. This approach accounts for potential tip shape imperfections that become more pronounced at different load levels.
  • Machine Stiffness Determination: They develop a method to determine the machine stiffness, also as a function of load. This is crucial because the machine stiffness is not constant and significantly impacts the measured displacements. Their approach leverages the calibrated effective tip radius and data from reference materials.
  • Integrated Workflow: The paper synthesizes these calibration steps into a single, iterative workflow. This workflow is validated against established benchmarks, such as a constant Young's modulus with depth, and consistent tip shape measurements across different reference materials.
  • Zero-Point Correction: They adapt a method for determining the zero-point of contact (initial load and displacement) by minimizing the residual between experimental data and a perfect elasticity model. This is particularly important for materials with short or noisy elastic loading segments.
  • Stress-Strain Curve Extraction: The calibrated parameters are then used to extract indentation stress-strain curves from materials with unknown moduli (tungsten, olivine, titanium).

Datasets

The study utilizes data from nanoindentation experiments performed on:

  • Reference Materials: Fused silica, sapphire, and glassy carbon. These materials have well-characterized elastic properties and are used for calibrating the effective tip radius and machine stiffness.
  • Materials with Unknown Moduli: Tungsten, titanium, and olivine. These are used to demonstrate the application of the developed calibration and analysis routines for extracting stress-strain curves and material properties.

The paper does not introduce new benchmark datasets but rather uses existing reference materials to validate its calibration procedures against known properties.

Key Insights and Ideas

  • Effective Radius is Load-Dependent: A critical insight is that the effective tip radius of a spherical indenter is not constant but varies with the applied load. This is attributed to tip shape imperfections and is crucial for accurate stress-strain curve extraction.
  • Machine Stiffness is Crucial and Load-Dependent: The instrument's own stiffness significantly influences measured displacements. Treating it as a constant can lead to errors, especially when comparing data across different instruments or load ranges.
  • Self-Consistent Calibration is Key: The paper emphasizes the importance of a self-consistent calibration routine where both effective radius and machine stiffness are determined simultaneously and iteratively, rather than relying on separate, potentially conflicting, measurements.
  • Impact on Yield Stress Identification: The accuracy of machine stiffness calibration directly impacts the identification of the yield point, highlighting the interconnectedness of these parameters.
  • Unified Workflow for Diverse Materials: The developed workflow is shown to be applicable to a range of materials with varying ductility, from brittle ceramics to ductile metals.

Key Results

  • The proposed calibration routine, which parameterizes the effective tip radius and machine stiffness as functions of load, leads to more consistent and reliable measurements.
  • Validation against benchmarks shows improved agreement in Young's modulus with depth and consistent effective tip shapes across different reference materials.
  • The application of the workflow to tungsten, titanium, and olivine successfully yielded indentation stress-strain curves.
  • The study demonstrates an indentation size effect in these materials, where yield stress increases with decreasing effective tip radius.
  • The method for zero-point correction, by minimizing the residual to an elasticity model, proved effective even for materials with short elastic segments.

Limitations and Future Work

  • Subjectivity in Elastic Segment Identification: While the zero-point correction method is improved, identifying the precise elastic loading segment for fitting can still be subjective, especially in materials with a very gradual transition to plasticity.
  • Linear Approximation for Machine Stiffness: The paper acknowledges that the linear fitting of machine stiffness as a function of load is a practical approximation, and that the actual relationship might be more complex.
  • Future Work: The authors suggest that future studies would benefit from detailed reports of calibration procedures and validation against benchmarks to ensure comparability of results. They also imply that further refinement of the zero-point correction and yield point identification methods could be beneficial, particularly for materials with complex deformation behaviors like pop-ins. The developed workflow is intended to be a guide for future studies aiming to extract and process data from spherical nanoindentation.

Summary updated

Abstract

Instrumented spherical nanoindentation with a continuous stiffness measurement has gained increased popularity in material science studies in brittle and ductile materials alike. These investigations span hypotheses related to a wide range of microphysics involving grain boundaries, twins, dislocation densities, ion-induced damage and more. These studies rely on the implementation of different methodologies for instrument calibration and for circumventing tip shape imperfections. In this study, we test, integrate, and re-adapt published strategies for tip and machine-stiffness calibration for spherical tips. We propose a routine for independently calibrating the effective tip radius and the machine stiffness using three reference materials (fused silica, sapphire, glassy carbon), which requires the parametrization of the effective radius as a function of load. We validate our proposed workflow against key benchmarks, such as variation of Young's modulus with depth. We apply the resulting calibrations to data collected in materials with varying ductility (olivine, titanium, and tungsten) to extract indentation stress-strain curves. We also test the impact of the machine stiffness on recently proposed methods for identification of yield stress, and compare the influence of different conventions on assessing the indentation size effect. Finally, we synthesize these analysis routines in a single workflow for use in future studies aiming to extract and process data from spherical nanoindentation.
BibTeX
@article{avadanii2023calibration,
  author = {Diana Avadanii and Anna Kareer and Lars Kai Hansen and A.J. Wilkinson},
  title = {{Calibration and data analysis routines for nanoindentation with spherical tips}},
  journal = {Journal of Materials research/Pratt's Guide to Venture Capital Sources},
  year = {2023},
}
Figure