Activation and failure mechanism of La0.6Sr0.4Co0.2Fe0.8O3−δ air electrode in solid oxide electrolyzer cells under high-current electrolysis

Zehua Pan, Qinglin Liu, Meng Ni, Renzhi Lyu, Ping Li, Siew Hwa ChanInternational Journal of Hydrogen Energy 2018 · DOI

Introduction

Solid Oxide Electrolyzer Cells (SOECs) represent a critical technology for high-efficiency hydrogen production, particularly when integrated with intermittent renewable energy sources. Among the various materials studied for air electrodes, $La_{0.6}Sr_{0.4}Co_{0.2}Fe_{0.8}O_{3-\delta}$ (LSCF) is widely regarded as a premier candidate due to its high mixed ionic-electronic conductivity (MIEC). However, the long-term stability of LSCF electrodes—especially when paired with industry-standard yttria-stabilized zirconia (YSZ) electrolytes—remains a significant hurdle. Under high-current electrolysis, these cells often suffer from catastrophic delamination, where the electrode physically separates from the electrolyte. This study investigates the chemical and physical mechanisms driving this failure, revealing a complex interplay between interfacial activation and mechanical degradation.

Experimental Methodology

To isolate the electrochemical behavior of the air electrode, researchers employed a half-cell configuration consisting of an LSCF working electrode, a YSZ electrolyte, and Platinum counter and reference electrodes. The study focused on two distinct sample types based on their thermal history:

  • Y1000: Sintered at 1000 °C, representing standard high-temperature processing conditions.
  • Y800: Sintered at 800 °C, a lower temperature intended to minimize deleterious interfacial reactions.

The investigation utilized Electrochemical Impedance Spectroscopy (EIS) and Distribution of Relaxation Times (DRT) to characterize electrical processes. Microstructural and chemical analyses were performed using Field Emission Scanning Electron Microscopy (FESEM), Energy Dispersive X-ray Spectroscopy (EDX), and X-ray Diffraction (XRD).

Results and Discussion

The Formation of the Interfacial Barrier

A primary finding of the study is the role of the sintering temperature in forming an interfacial secondary phase. In the Y1000 samples, high-temperature processing leads to the formation of a thin (~100 nm), dense layer of Strontium Zirconate ($SrZrO_3$) at the LSCF/YSZ interface. Because $SrZrO_3$ is an electrical insulator, these cells initially exhibit very high ohmic and polarization resistance.

The Activation Mechanism: Cobalt Diffusion

Interestingly, the Y1000 cells demonstrated a significant "activation" period during the first 18 hours of electrolysis, where polarization resistance dropped from $1.53 \Omega cm^2$ to much lower levels. This improvement was traced to the diffusion of Cobalt (Co) from the LSCF electrode into the $SrZrO_3$ layer. EDX analysis confirmed that after only 30 minutes of operation, the Cobalt content at the interface increased from 0% to approximately 8 at.%. This "infiltration" of Cobalt renders the previously insulating $SrZrO_3$ layer more ionically conductive and catalytically active, temporarily boosting cell performance.

The Failure Mechanism: Oxygen Trapping and Delamination

The activation of the interface, however, creates a "pressure cooker" effect. As the $SrZrO_3$ layer becomes more active, oxygen gas is generated at the interface between the $SrZrO_3$ and the YSZ electrolyte. Because the $SrZrO_3$ layer is dense and lacks sufficient porosity, the evolved oxygen gas cannot escape through the electrode.

As electrolysis continues at high current densities, the internal gas pressure at the interface builds up. Eventually, this mechanical stress exceeds the adhesive strength of the interface, causing the $SrZrO_3$ layer—and the LSCF electrode attached to it—to delaminate from the YSZ electrolyte. This process explains the characteristic performance curve of Y1000 cells: a period of improving performance (activation) followed by a sharp spike in resistance (failure) as the physical contact is lost.

Comparative Stability

In contrast, the Y800 samples, which were sintered at a lower temperature to avoid the formation of the $SrZrO_3$ layer, showed stable performance throughout the testing period. These cells did not exhibit the activation-then-failure cycle, nor did they show signs of delamination, confirming that the $SrZrO_3$ secondary phase is the root cause of the mechanical instability.

Conclusion and Implications

This research highlights a dual-role for Cobalt in LSCF/YSZ systems: while it facilitates the activation of resistive interfacial layers, it simultaneously accelerates the conditions leading to delamination. The findings suggest that preventing the formation of $SrZrO_3$ is paramount for SOEC longevity.

While Gadolinium-doped Ceria (GDC) buffer layers are often used to prevent such reactions, the "oxygen trapping" mechanism identified here may still occur if secondary phases form over extended operational lifetimes. Consequently, the study points toward two primary engineering solutions: either developing low-temperature fabrication techniques to bypass the formation of insulating secondary phases entirely, or transitioning toward Cobalt-free air electrode materials to eliminate the diffusion-driven activation/failure cycle.

Summary updated

BibTeX
@article{pan2018activation,
  author = {Zehua Pan and Qinglin Liu and Meng Ni and Renzhi Lyu and Ping Li and Siew Hwa Chan},
  title = {{Activation and failure mechanism of La0.6Sr0.4Co0.2Fe0.8O3−δ air electrode in solid oxide electrolyzer cells under high-current electrolysis}},
  journal = {International Journal of Hydrogen Energy},
  year = {2018},
  doi = {10.1016/j.ijhydene.2018.01.181},
}
Figure