3D characterisation of hydrogen environmentally assisted cracking during static loading of AA7449-T7651

Unai De Francisco, Felix Beckmann, Julian Moosmann, N.o. Larrosa, Matthew PeelInternational Journal of Fracture 2021 · DOI

Abstract

In this investigation, synchrotron X-ray microtomography was used to perform 3D in situ observations of crack initiation and growth during hydrogen environmentally assisted cracking (HEAC) in tensile samples of AA7449-T7651. Two smooth tensile samples with a 1 mm diameter gauge section were held at a fixed displacement (~30% of yield stress) in warm, moist air (~76°C, 73% relative humidity). The samples were then imaged repeatedly using X-ray tomography until they fractured completely. The tomograms showing the nucleation and evolution of intergranular cracks were correlated with electron microscopy fractographs. This enabled the identification of crack initiation sites and the characterisation of the crack growth behaviour relative to the microstructure. The samples were found to fracture within an environmental exposure time of 240 min. Some cracks in both samples nucleated within an exposure time of 80 min (33–40% of the total lifetime). Many cracks were found to nucleate both internally and at the sample surface. However, only superficial cracks contributed to the final fracture surface as they grew faster owing to the direct environmental exposure and the larger crack opening. HEAC occurred prominently via brittle intergranular cracking, and cracks were found to slow down when approaching grain boundary triple junctions. Additionally, crack shielding from nearby cracks and the presence of coarse Al–Cu–Fe particles at the grain boundaries were also found to temporarily reduce the crack growth rates. After prolonged crack growth, the HEAC cracks displayed ductile striations and transgranular fracture, revealing a change in the crack growth mechanism at higher stress intensity factors.

Introduction

High-strength 7xxx series aluminum alloys (Al-Zn-Mg-Cu) are foundational to modern aerospace structures. However, these materials exhibit a significant vulnerability to Hydrogen Environmentally Assisted Cracking (HEAC). When exposed to moisture, hydrogen atoms diffuse into the metal, embrittling grain boundaries and initiating cracks under static loads far below the material's yield strength. Historically, studying HEAC has been limited by 2D surface observations, which fail to capture the subsurface nucleation and the dynamic competition between multiple growing cracks.

Experimental Methodology

To address these limitations, researchers employed in situ synchrotron X-ray microtomography at the PETRA III beamline (DESY, Germany). This technique allowed for the real-time 3D tracking of crack evolution with a spatial resolution of 0.5 µm.

Schematic of the tensile sample geometry (a) and the specific 1 mm diameter gauge section (b) used for in situ environmental testing.

Samples were placed in a custom environmental rig, held under static tension (~30% yield stress), and exposed to warm, moist air (76°C, 73% RH). Full 3D tomograms were captured every few minutes, and machine learning-based segmentation (3D WEKA) was used to distinguish cracks from the aluminum matrix and intermetallic particles.

Key Insights and Microstructural Interactions

Nucleation and Growth Dynamics

Cracks were observed to nucleate both internally and at the surface within the first 80 minutes. However, surface cracks became the primary drivers of failure, growing exponentially faster due to direct environmental access and larger crack mouth opening displacements (CMOD).

Microstructural Sensitivity

A critical finding was the role of recrystallized grains in crack initiation. Approximately 45–70% of the cracks that led to final failure originated at the interfaces of these grains, identifying them as particularly vulnerable regions within the AA7449-T7651 microstructure.

Micrograph highlighting recrystallised grains (orange) within the alloy, showing their orientation relative to the short-transverse (ST) and longitudinal (L) directions.

Propagation Obstacles

The study identified several features that act as temporary "speed bumps" for HEAC:

  • Triple Junctions: Cracks often paused or slowed at the intersection of three grains.
  • Intermetallic Particles: Coarse Al–Cu–Fe particles at grain boundaries forced cracks to propagate around them.
  • Crack Shielding: Proximity between multiple cracks reduced local mechanical stress, paradoxically slowing individual growth rates.

Results and Mechanism Transition

Samples reached complete fracture within 200–240 minutes. The lateral growth of the fractured area followed an exponential trend, with crack densities reaching up to 98 cracks/mm³ in high-stress regions. As the cracks propagated and the stress intensity factor ($K_I$) increased beyond approximately 2.8 MPa√m, the fracture mode transitioned from brittle intergranular cracking to ductile transgranular fracture, evidenced by the appearance of striations.

Conclusion

This research provides unprecedented 3D insights into the "birth" and progression of hydrogen-induced cracks in aerospace aluminum. By quantifying the influence of microstructural features like recrystallized grains and intermetallic particles, the study offers a clearer roadmap for developing more crack-resistant alloys. Future work will focus on thicker samples to better simulate the conditions found in large-scale aircraft components.

Reference: De Francisco, U., Beckmann, F., Moosmann, J. et al. 3D characterisation of hydrogen environmentally assisted cracking during static loading of AA7449-T7651. Int J Fract (2021). https://doi.org/10.1007/s10704-021-00595-y

Summary updated

Abstract

Abstract In this investigation, synchrotron X-ray microtomography was used to perform 3D in situ observations of crack initiation and growth during hydrogen environmentally assisted cracking (HEAC) in tensile samples of AA7449-T7651. Two smooth tensile samples with a 1 mm diameter gauge section were held at a fixed displacement ( $$\approx 30$$ <mml:math xmlns:mml="http://www.w3.org/1998/Math/MathML"> <mml:mrow> <mml:mo>≈</mml:mo> <mml:mn>30</mml:mn> </mml:mrow> </mml:math> % of yield stress) in warm, moist air ( $$\approx 76\,^\circ $$ <mml:math xmlns:mml="http://www.w3.org/1998/Math/MathML"> <mml:mrow> <mml:mo>≈</mml:mo> <mml:mn>76</mml:mn> <mml:msup> <mml:mspace/> <mml:mo>∘</mml:mo> </mml:msup> </mml:mrow> </mml:math> C, 73% relative humidity). The samples were then imaged repeatedly using X-ray tomography until they fractured completely. The tomograms showing the nucleation and evolution of intergranular cracks were correlated with electron microscopy fractographs. This enabled the identification of crack initiation sites and the characterisation of the crack growth behaviour relative to the microstructure. The samples were found to fracture within an environmental exposure time of 240 min. Some cracks in both samples nucleated within an exposure time of 80 min (33–40% of the total lifetime). Many cracks were found to nucleate both internally and at the sample surface. However, only superficial cracks contributed to the final fracture surface as they grew faster owing to the direct environmental exposure and the larger crack opening. HEAC occurred prominently via brittle intergranular cracking, and cracks were found to slow down when approaching grain boundary triple junctions. Additionally, crack shielding from nearby cracks and the presence of coarse Al–Cu–Fe particles at the grain boundaries were also found to temporarily reduce the crack growth rates. After prolonged crack growth, the HEAC cracks displayed ductile striations and transgranular fracture, revealing a change in the crack growth mechanism at higher stress intensity factors.
BibTeX
@article{francisco2021d,
  author = {Unai De Francisco and Felix Beckmann and Julian Moosmann and N.O. Larrosa and Matthew Peel},
  title = {{3D characterisation of hydrogen environmentally assisted cracking during static loading of AA7449-T7651}},
  journal = {International Journal of Fracture},
  year = {2021},
  doi = {10.1007/s10704-021-00595-y},
}
Figure